MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

EMS-Grivory Grilamid® 2D 20 nat PA612
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 612 (PA612)

Material Notes: Product Description: Grilamid 2D 20 natural is an unmodified unreinforced, medium viscosity polyamide 612 (PA612), designed for injection molding as well as extrusion. It is characterized by the following product profile:
  • Good chemical resistance
  • Moderate water absorption
  • High strength
  • Ductile, resilient in conditioned stage
  • Low density
Grilamid 2D 20 natural is suitable for applications at moderate continuous use temperatures and without repeated direct exposure to UV radiation. Preferred applications:
  • Injection molded functional parts
  • Bushes, gears
  • Semi-fabricates such as tubes, film, sheet, profiles
  • Sheathing guides

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.06 g/cc0.0383 lb/in³Dry; ISO 1183
Water Absorption 2.8 %2.8 %Sim. to ISO 62
Moisture Absorption 1.30 %1.30 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.017 cm/cm0.017 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.017 cm/cm0.017 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D  76
@Time 15.0 sec
76
@Time 0.00417 hour
Conditioned; ISO 868
 81
@Time 15.0 sec
81
@Time 0.00417 hour
Dry; ISO 868
Tensile Strength, Yield 50.0 MPa7250 psiConditioned; ISO 527-1/-2
 60.0 MPa8700 psiDry; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Nominal, Dry; ISO 527-1/-2
 >= 50 %>= 50 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 4.0 %4.0 %Dry; ISO 527-1/-2
 16 %16 %Conditioned; ISO 527-1/-2
Tensile Modulus 1.60 GPa232 ksiConditioned; ISO 527-1/-2
 2.30 GPa334 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+8 ohm-cm1.00e+8 ohm-cmDry; IEC 60093
 1.00e+8 ohm-cm1.00e+8 ohm-cmConditioned; IEC 60093
Surface Resistance 1.00e+10 ohm1.00e+10 ohmIEC 60093
Dielectric Strength 32.0 kV/mm813 kV/inDry; IEC 60243-1
 32.0 kV/mm813 kV/inConditioned; IEC 60243-1
Comparative Tracking Index 600 V600 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.1 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C50.0 µin/in-°FISO 11359-1/-2
Melting Point 218 °C424 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 80.0 °C176 °FLong Term; ISO 2578
 150 °C302 °FShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 130 °C266 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
FormGranules
Industry & Consumer goodsHousewares
 Mechanical Engineering
 Tools & Accessories
ProcessingFilm Extrusion
 Other Extrusion
Product AttributesHigh viscosity

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® 1503-2 NF2004 33% Glass Filled PA66 (Conditioned)
BASF Ultramid® 8202 PA6 (Conditioned)
304 Stainless Steel
BASF Ultramid® 1000-11 NF2001 PA66 (Conditioned)
BASF Ultramid® 8233G HS 33% Glass Filled PA6 (Dry)

PGRH008 / 156717

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.