MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil SpectraSyn Elite™ 300 Metallocene Polyalphaolefin Fluid
Categories: Fluid; Lubricant; Polyalphaolefin (PAO)

Material Notes: SpectraSyn Elite™ metallocene polyalphaolefin (mPAO) advanced synthetic base oil is a high-performance polyalphaolefin (PAO) designed to provide better blending efficiency and performance capabilities than conventional synthetic PAO. SpectraSyn Elite mPAO base oil offers formulators the flexibility to develop innovative finished lubricants to help meet the growing demand for energy efficiency and product durability. Available in 65, 150 and 300 cSt at 100°C, SpectraSyn Elite mPAO is created using proprietary metallocene catalyst technology. Particularly well-suited for industrial oils requiring high stability under severe operating conditions, SpectraSyn Elite mPAO base oil can be used in combination with lower-viscosity fluids (PAO, mineral oils) to achieve a wide range of industrial and automotive lubricants and greases. Benefits: Viscosity index range, for high performance at a wide temperature range, Shear stability, for long drain intervals, Low-temperature properties, for cold-start capability and fluidity.

Availability: Africa & Middle East, Europe, North America, Asia Pacific, Latin America. Appearance: Bright & Clear.

Information provided by ExxonMobil.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.849 g/cc
@Temperature 15.6 °C
0.0307 lb/in³
@Temperature 60.1 °F
ASTM D4052
Viscosity Measurement 241241Viscosity Index; ASTM D2270
Kinematic Viscosity 3358 cSt
@Temperature 40.0 °C
3358 cSt
@Temperature 104 °F
ASTM D445
Kinematic Viscosity at 100°C (212°F) 303 cSt
@Temperature 100 °C
303 cSt
@Temperature 212 °F
ASTM D445
ASTM Color <= 0.50<= 0.50ASTM D1500/D6045
 
Chemical PropertiesMetricEnglishComments
Total Acid Number <= 0.10<= 0.10mg KOH/g; ASTM D974
 
Thermal PropertiesMetricEnglishComments
Pour Point -32.8 °C-27.0 °FASTM D5950/D97
Flash Point 286 °C547 °FCOC; ASTM D92
 
Component Elements PropertiesMetricEnglishComments
H2O, Water <= 0.0050 %<= 0.0050 %ASTM D6304

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil SpectraSyn Ultra™ 300 High VI Polyalphaolefin (PAO) Fluid
ExxonMobil SpectraSyn Ultra™ 1000 High VI Polyalphaolefin (PAO) Fluid
ExxonMobil SpectraSyn Elite™ 150 Metallocene Polyalphaolefin (mPAO) Fluid
ExxonMobil Mobilgear SHC Series 680
ChevronTexaco Cetus® PAO 100

PEX98990 / 238371

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.