MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

American Maple, Rock (Sugar Maple)
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: High resistance to abrasion. Diffuse-Porous Hardwood. Least easy to work with hand tools. Excellent shaping, fair planing, fair steam bending. Data is based on small, clear, air-dried samples unless specified.
Usual surface texture: Fine
Dimensional changes when dried lumber is subjected to variations in humidity during service: Medium
Resistance to fungal decay (Heartwood in ground contact): Non-durable (5 to 10 years)
Resistance to penetration by preservatives: Resistant
Common Applications: Excellent flooring timber. Furniture. Sports goods

Property values marked by an asterisk (*) have been taken from an unusually old reference source.

Key Words: Acer saccharum; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.570 g/cc0.0206 lb/in³Oven Dry Weight/Unseasoned Volume
 0.897 g/cc0.0324 lb/in³Unseasoned*
Cell Length 0.800 mm0.0315 inMature Wood
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 4000 N899 lb (f)Side. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 4400 N989 lb (f)End. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 6400 N1440 lb (f)Side
Tensile Strength, Ultimate 5.31 MPa770 psiPerpendicular to Grain*
Modulus of Rupture 0.0627 GPa9.10 ksiStatic Bending*
 0.109 GPa15.8 ksiIn Bending
Flexural Yield Strength 34.5 MPa5000 psiFiber Stress at Elastic Limit; Static Bending*
 65.5 MPa9500 psiBending stress at proportional limit
Flexural Modulus 10.2 GPa1480 ksiStatic Bending*
 12.4 - 12.63 GPa1800 - 1832 ksiIn Bending
Compressive Strength 5.17 MPa750 psiPerpendicular to Grain*
 12.5 MPa1810 psiPerpendicular to Grain
 21.5 MPa3120 psiParallel to Grain*
 26.6 MPa3860 psiMax Crushing Strength Parallel to Grain*
 53.8 - 54.0 MPa7800 - 7830 psiParallel to Grain
Poissons Ratio 0.0370.037µTL, 12% Moisture Content
 0.0650.065µRL, 12% Moisture Content
 0.3490.349µTR, 12% Moisture Content
 0.4240.424µLR, 12% Moisture Content
 0.4760.476µLT, 12% Moisture Content
 0.7740.774µRT, 12% Moisture Content
Machinability 50 %50 %Medium Relative to Other Wood
Shear Strength 9.51 MPa1380 psiParallel to Grain*
 16.1 MPa2340 psiOrientation Unknown
Impact 5.05.0in-lb/in³; Work to Elastic Limit; Unseasoned Sample; Impact Bending*
 1210012100psi; Fiber Stress at Elastic Limit; Unseasoned Sample; Impact Bending*
Work to Elastic Limit 0.00745 J/cm³1.08 in-lb/in³Static Bending*
Work to Maximum Load 0.0820 J/cm³11.9 in-lb/in³Static Bending*
Toughness 40.7 J30.0 ft-lbTangential
 41.8 J30.8 ft-lbRadial
Cleavage 66.0 kN/m377 lb/inRadial surface of failure, Unseasoned*
 90.0 kN/m514 lb/inTangential surface of failure, Unseasoned*
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.0288 W/m-K0.200 BTU-in/hr-ft²-°F12% Moisture Content
 0.144 W/m-K1.00 BTU-in/hr-ft²-°FOven Dry
Shrinkage 4.9 %4.9 %Radial; Green to Zero Moisture
 9.5 %9.5 %Tangential; Green to Zero Moisture
 14.9 %14.9 %Volumetric; Green to Zero Moisture
 
Descriptive Properties
ColorCreamy whiteUsual for heartwood

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
American Yellow Birch Wood
Paper Birch Wood
Sweet Birch Wood
Black Maple Wood
Bigleaf Maple Wood

PTSAU / 71304

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.