MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

General Plastics LAST-A-FOAM® FR-6720 Polyurethane Foam
Categories: Other Engineering Material; Composite Core Material; Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane Foam, Unreinforced

Material Notes: Product Description: LAST-A-FOAM® FR-6700 is a CFC-free, rigid, closed-cell, flame-retardant polyurethane foam for aircraft composite core that withstands process temperatures up to 250°F. It is available in densities ranging from 10 to 25 pounds per cubic foot and exhibits a high strength-to-weight ratio due to its cellular structure and cross-linked resin. Because of its closed-cell structure, LAST-A-FOAM® FR-6700 has great resistance to water absorption and will not swell, crack, or split on exposure to water.

Product Feature:

  • Stable
  • Inert
  • Will not support fungal growth
  • Resistant to most chemicals and solvents
  • Easily shaped with common woodworking tools
  • Performs well as wood replacement
Applications:
  • Models and design prototypes
  • Composite Core
  • Honeycomb edge close-out for aircraft interior sandwich panels used in overhead storage bins, passenger cabin class dividers, galleys and lavatories
  • Vacuum form dies and mold patterns

Information provided by General Plastics Manufacturing Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.320 g/cc0.0116 lb/in³ASTM D1622
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 35.635.6cut foam surface; ASTM D2240
Tensile Strength 5.47 MPa793 psiPerpendicular to Rise; ASTM D1623
 5.52 MPa801 psiParallel to Rise; ASTM D1623
Flexural Strength 8.439 MPa1224 psiRise Parallel to Beam Thick.; ASTM D790
 8.453 MPa1226 psiRise Parallel to Test Span; ASTM D790
Flexural Modulus 0.29215 GPa42.373 ksiRise Parallel to Test Span; ASTM D790
 0.29888 GPa43.349 ksiRise Parallel to Beam Thick.; ASTM D790
Compressive Strength  3.50 MPa
@Temperature 121 °C
508 psi
@Temperature 250 °F
Parallel to Rise; ASTM D1621
 3.75 MPa
@Temperature 121 °C
544 psi
@Temperature 250 °F
Perpendicular to Rise; ASTM D1621
 5.52 MPa
@Temperature 93.3 °C
801 psi
@Temperature 200 °F
Parallel to Rise; ASTM D1621
 5.55 MPa
@Temperature 93.3 °C
805 psi
@Temperature 200 °F
Perpendicular to Rise; ASTM D1621
 9.598 MPa
@Temperature 23.9 °C
1392 psi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
 9.639 MPa
@Temperature 23.9 °C
1398 psi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
 14.73 MPa
@Temperature -53.9 °C
2136 psi
@Temperature -65.0 °F
Perpendicular to Rise; ASTM D1621
 14.83 MPa
@Temperature -53.9 °C
2151 psi
@Temperature -65.0 °F
Parallel to Rise; ASTM D1621
Compressive Modulus  0.12008 GPa
@Temperature 121 °C
17.416 ksi
@Temperature 250 °F
Parallel to Rise; ASTM D1621
 0.12009 GPa
@Temperature 121 °C
17.417 ksi
@Temperature 250 °F
Perpendicular to Rise; ASTM D1621
 0.17183 GPa
@Temperature 93.3 °C
24.922 ksi
@Temperature 200 °F
Parallel to Rise; ASTM D1621
 0.17307 GPa
@Temperature 93.3 °C
25.102 ksi
@Temperature 200 °F
Perpendicular to Rise; ASTM D1621
 0.24408 GPa
@Temperature 23.9 °C
35.401 ksi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
 0.25344 GPa
@Temperature 23.9 °C
36.759 ksi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
 0.27737 GPa
@Temperature -53.9 °C
40.229 ksi
@Temperature -65.0 °F
Perpendicular to Rise; ASTM D1621
 0.28153 GPa
@Temperature -53.9 °C
40.832 ksi
@Temperature -65.0 °F
Parallel to Rise; ASTM D1621
Poissons Ratio 0.300.30
 
Thermal PropertiesMetricEnglishComments
CTE, linear  72.0 µm/m-°C
@Temperature 23.9 - 121 °C
40.0 µin/in-°F
@Temperature 75.0 - 250 °F
 630 µm/m-°C
@Temperature -45.6 - 93.3 °C
350 µin/in-°F
@Temperature -50.0 - 200 °F
GP Method
Specific Heat Capacity 1.57 J/g-°C0.376 BTU/lb-°FASTM E1269
Thermal Conductivity 0.0584 W/m-K0.405 BTU-in/hr-ft²-°FASTM C518
Maximum Service Temperature, Air 121 °C250 °F
Minimum Service Temperature, Air -196 °C-320 °F
Glass Transition Temp, Tg 135 °C275 °FASTM E1824
 
Descriptive Properties
Closed Cell Content68%25 lbs/ft3
 96%10 lbs/ft3
Heat of Combustion10939 BTU/lbASTM D240
Tumbling Friability (%)125 lbs/ft3
 10.8910 lbs/ft3
Water Absorption0.01 lbs/ft²18 lbs/ft³
 0.049 lbs/ft²10 lbs/ft³

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
General Plastics LAST-A-FOAM® FR-6718 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-3703 Polyurethane Foam
BCC Products MB 1200 Polyurethane Foam Modeling Board
Covestro Baynat® 3002 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-3706 Polyurethane Foam

PGENR040 / 186826

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.