MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay CYFORM® 22 Epoxy Tooling Prepreg
Categories: Polymer; Thermoset; Epoxy

Material Notes: Description: CYFORM 22 is a proven, high-performance and cost-effective, low-temperature-curing epoxy tooling system available with either carbon or glass reinforcement. CYFORM 22 allows high-quality tooling laminates to be produced directly from a low-temperature master model. After vacuum bag/oven or autoclave processing for the initial cure, the tool laminate can be de-molded and post-cured “free-standing”. CYFORM 22 is supplied in roll form with a standard roll length of 25 yards (25 meters). Standard material width is 50 inches (1000 – 1270mm). Materials are shipped frozen and in insulated boxes.

Features & Benefits:

  • Provides versatile low temperature curing options from 7 days at 68°F (20°C) to 5 hours at 130°F (55°C)
  • Manufactured to ensure uniform resin distribution in fabrics with <1% volatile content
  • Formulated for long-term thermal oxidative stability during normal 350°F (177°C) service
  • Exhibits low and predictable shrinkage with both carbon and glass fiber reinforcement
  • Closely matches the thermal expansion coefficient of composite parts reducing dimensional inaccuracies and residual stress levels
  • When used with a surface gel coat, produces tools of extremely low void content via vacuum-bag-only processing if autoclave facilities are not available
  • Determined safe to use via extensive toxicological screening (contains no MDA or VCHDs)
Suggested Applications:
  • Tools used for manufacture of composite components where the master model is made of high-CTE material
  • Ideally suited for the rapid manufacture of complex mold tooling; e.g., Formula 1 race cars

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Volatiles <= 1.0 %<= 1.0 %Carbon
 <= 1.0 %<= 1.0 %Glass
 
Mechanical PropertiesMetricEnglishComments
Flexural Modulus  16.0 GPa
@Temperature 177 °C
2320 ksi
@Temperature 351 °F
GPT, After post-cure
 17.0 GPa
@Temperature 177 °C
2470 ksi
@Temperature 351 °F
GPT, After thermal cycling
 23.0 GPa
@Temperature 90.0 °C
3340 ksi
@Temperature 194 °F
GPT, After post-cure
 26.0 GPa
@Temperature 20.0 °C
3770 ksi
@Temperature 68.0 °F
GPT, After post-cure
 26.0 GPa
@Temperature 20.0 °C
3770 ksi
@Temperature 68.0 °F
GPT, After thermal cycling
 35.0 GPa
@Temperature 177 °C
5080 ksi
@Temperature 351 °F
CP200, After thermal cycling
 38.0 GPa
@Temperature 177 °C
5510 ksi
@Temperature 351 °F
CP200, After post-cure
 41.0 GPa
@Temperature 20.0 °C
5950 ksi
@Temperature 68.0 °F
CP200, After thermal cycling
 45.0 GPa
@Temperature 90.0 °C
6530 ksi
@Temperature 194 °F
CP200, After post-cure
 46.0 GPa
@Temperature 20.0 °C
6670 ksi
@Temperature 68.0 °F
CP200, After post-cure
 
Thermal PropertiesMetricEnglishComments
CTE, linear 2.50 µm/m-°C1.39 µin/in-°FCarbon
 14.6 µm/m-°C8.11 µin/in-°FGlass
Maximum Service Temperature, Air 177 °C351 °Flong-term
Glass Transition Temp, Tg 204 °C399 °FCarbon
 204 °C399 °FGlass
Shrinkage 0.031 %0.031 %Carbon
 0.15 %0.15 %Glass
 
Processing PropertiesMetricEnglishComments
Gel Time  8.00 min
@Temperature 40.0 °C
8.00 min
@Temperature 104 °F
Carbon
 8.00 min
@Temperature 40.0 °C
8.00 min
@Temperature 104 °F
Glass
 108 min
@Temperature 20.0 °C
108 min
@Temperature 68.0 °F
Carbon
 108 min
@Temperature 20.0 °C
108 min
@Temperature 68.0 °F
Glass
Shelf Life  6.00 Month
@Temperature -18.0 °C
6.00 Month
@Temperature -0.400 °F
Carbon
 6.00 Month
@Temperature -18.0 °C
6.00 Month
@Temperature -0.400 °F
Glass

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay LTS90B/G Sealant tape
Solvay CYCOM® 381 Epoxy Prepreg with E-glass Fabric and 300FAW Epoxy
Solvay CYCOM® 381 Epoxy Prepreg with CYCOM 7781 OST E-glass Fabric and 300FAW Epoxy
Solvay CYCOM® 381 Epoxy E-glass Prepreg
Lord Adhesives Circalok™ EP-729 Epoxy Board Level Encapsulant

PCYTED189 / 180491

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.