MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

BASF Nypel® 6015G HS BK 15% Glass Filled PA6 (Dry)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Glass Fiber Filled

Material Notes: Nypel 6015G HS BK is a 15% glass reinforced, heat stabilized injection molding compound. It offers good mechanical properties with excellent processability.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.23 g/cc0.0444 lb/in³ISO 1183
Water Absorption 1.4 %1.4 %24 hour; ISO Test
 8.2 %8.2 %ISO 62
Moisture Absorption at Equilibrium 2.3 %2.3 %23°C/50% R.H.; ISO 62
Viscosity Measurement 6161Formic Acid
Linear Mold Shrinkage 0.0050 cm/cm0.0050 in/inASTM Data; MD
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 121121ASTM Test
Tensile Strength at Break 120 MPa17400 psi0.2 in/min; ASTM Test
Tensile Strength, Ultimate 110 MPa16000 psi5mm/min; ISO 527
Elongation at Break 2.0 %2.0 %5mm/min; ISO 527
 3.0 %3.0 %0.2 in/min; ASTM Test
Tensile Modulus 5.70 GPa827 ksi1mm/min; ISO 527
Flexural Strength 165 MPa23900 psiISO Data
Flexural Modulus 4.80 GPa696 ksiISO Data
 5.38 GPa780 ksiASTM Test
Izod Impact, Notched 0.450 J/cm
@Thickness 3.17 mm
0.843 ft-lb/in
@Thickness 0.125 in
ASTM Test
Izod Impact, Notched (ISO) 4.50 kJ/m²2.14 ft-lb/in²ISO Test
 4.00 kJ/m²
@Temperature -40.0 °C
1.90 ft-lb/in²
@Temperature -40.0 °F
ISO Test
Charpy Impact Unnotched 3.00 J/cm²14.3 ft-lb/in²ISO 179
Charpy Impact, Notched 0.400 J/cm²1.90 ft-lb/in²ISO 179
 0.300 J/cm²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 
Thermal PropertiesMetricEnglishComments
CTE, linear 50.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
27.8 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM Test
Melting Point 220 °C428 °F10 K/min
 220 °C428 °FASTM Test
Deflection Temperature at 0.46 MPa (66 psi) 210 °C410 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 190 °C374 °FISO 75
 200 °C392 °FASTM Test
Flammability, UL94  HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 
Descriptive Properties
ColorBK
Commercial StatusActive America
Impact ModifiedNo
Primary Processing TechniqueInjection Molding
ProcessingInjection Molding
UL.UL-CYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Nypel® 6030G HS BK 30% Glass Filled PA6 (Dry)
BASF Capron® 8200 NL Nylon 6 (DAM)
BASF Capron® 8200 NL Nylon 6 (Conditioned)
BASF Ultramid® 8202 PA6 (Conditioned)
BASF Ultramid® B3ZG3 15% Glass Filled PA6 (Dry)

PBASF9012 / 84776

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.