MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Makrolon® FR 6002 Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: Makrolon® is extremely robust, lightweight with glass-like transparency and is impact resistant – even at extremely low temperatures. It has a high dimensional stability and is easily molded, yet has excellent heat resistance with a glass transition temperature of up to 148ºC. Grades are available optimized for lighting, medical and food contact, flame-retardant, impact-modified and glass-fiber reinforced grades. Products made out of polycarbonate boast a long life and allow efficient reusability. Stronger and lighter than glass, polycarbonate also provides energy and CO2 emission savings. Furthermore, it reduces product losses due to breakage during distribution and use. Most post-production waste is mechanically recycled into “recyclate grade” polycarbonate blends.

Mechanical property data for samples at 50% RH.

Information provided by Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ISO 1183-1
Melt Flow 21.6 g/10 min
@Load 1.20 kg,
Temperature 300 °C
21.6 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 65.0 MPa9430 psi50mm/min; ISO 527-1,-2
Tensile Strength, Yield 64.0 MPa9280 psi50mm/min; ISO 527-1,-2
Elongation at Break >= 50 %>= 50 %50mm/min, complete break; ISO 524-1,-2
 120 %120 %50mm/min, complete break; ISO 524-1,-2
Elongation at Yield 6.0 %6.0 %50mm/min; ISO 527-1,-2
Tensile Modulus 2.35 GPa
@Temperature 23.0 °C
341 ksi
@Temperature 73.4 °F
1mm/min, complete break; ISO 527-1,-2
Izod Impact, Notched (ISO) 15.0 kJ/m²
@Thickness 3.00 mm,
Temperature 23.0 °C
7.14 ft-lb/in²
@Thickness 0.118 in,
Temperature 73.4 °F
Complete Break; ISO 7391/b.o. ISO 180-A
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179-1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179-1eU
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.50e+17 ohm-cm1.50e+17 ohm-cmIEC 60093
Surface Resistance 4.20e+16 ohm4.20e+16 ohmIEC 60093
Dielectric Constant  2.9
@Frequency 1e+6 Hz
2.9
@Frequency 1e+6 Hz
IEC 60250
 3.0
@Frequency 100 Hz
3.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 34.0 kV/mm
@Thickness 1.00 mm
864 kV/in
@Thickness 0.0394 in
IEC 60243-1
Dissipation Factor  0.00080
@Frequency 100 Hz
0.00080
@Frequency 100 Hz
IEC 60250
 0.0088
@Frequency 1e+6 Hz
0.0088
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 125 V125 Vsolution B; IEC 60112
 250 V250 Vsolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 137 °C279 °Fcomplete break; ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 124 °C255 °Fcomplete break; ISO 75-1,-2
Vicat Softening Point 143 °C
@Load 5.10 kg
289 °F
@Load 11.2 lb
@ 50°C/h; ISO 306
UL RTI, Electrical 120 °C
@Thickness 1.50 mm
248 °F
@Thickness 0.0591 in
UL RTI, Mechanical with Impact 110 °C
@Thickness 1.50 mm
230 °F
@Thickness 0.0591 in
UL RTI, Mechanical without Impact 120 °C
@Thickness 1.50 mm
248 °F
@Thickness 0.0591 in
Flammability, UL94  V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
UL 94
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
UL 94
 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
UL 94
Oxygen Index >= 32 %>= 32 %ISO 4589-2
Glow Wire Ignition Temperature  850 °C
@Thickness 0.750 mm
1560 °F
@Thickness 0.0295 in
IEC 60695-2-13
 850 °C
@Thickness 1.50 mm
1560 °F
@Thickness 0.0591 in
IEC 60695-2-13
 930 °C
@Thickness 3.00 mm
1710 °F
@Thickness 0.118 in
IEC 60695-2-13
Glow Wire Flammability Index  960 °C
@Thickness 0.750 mm
1760 °F
@Thickness 0.0295 in
IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
1760 °F
@Thickness 0.0591 in
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
1760 °F
@Thickness 0.118 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 °C536 °Finjection molding; ISO 294
Mold Temperature 80.0 °C176 °Finjection molding; ISO 294
Injection Velocity 200 mm/sec7.87 in/secinjection molding; ISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Makrolon® 6265X Polycarbonate
Covestro Makrolon® ET IR320 Polycarbonate
Covestro Makrolon® FR 7087 Polycarbonate
Covestro Makrolon® 6267X Polycarbonate
Covestro Makrolon® ET 3113 Polycarbonate

PB095070 / 200140

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.