MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Outokumpu 253MA® High Temperature Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Variant of 1.4828 with increased nitrogen content and has been microalloyed with rare earth metals (REM). The most suitable temperature range is 850-1100°C, because structural changes when used between 600-850°C can lead to reduced impact toughness at room temperature.

Applications: Heat and creep resistance. For use over 550°C for equipment and components within:

  • Iron, steel, and non-ferrous industries
  • Engineering industry
  • Energy conservation plants
  • Cement industry

Available in hot rolled plate (Quarto), hot rolled strip/sheet (CPP), cold rolled strip/sheet, cold rolled narrow strip, bar, and rod forms.

Key Words: EN 1.4835; ASTM S30815
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³RT
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 700 MPa102000 psiOutokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 360 MPa
@Temperature 700 °C
52200 psi
@Temperature 1290 °F
EN min.
 445 MPa
@Temperature 600 °C
64500 psi
@Temperature 1110 °F
EN min.; EN 10002-5
 495 MPa
@Temperature 500 °C
71800 psi
@Temperature 932 °F
EN min.; EN 10002-5
 530 MPa
@Temperature 400 °C
76900 psi
@Temperature 752 °F
EN min.; EN 10002-5
 535 MPa
@Temperature 300 °C
77600 psi
@Temperature 572 °F
EN min.; EN 10002-5
 545 MPa
@Temperature 200 °C
79000 psi
@Temperature 392 °F
EN min.; EN 10002-5
 585 MPa
@Temperature 100 °C
84800 psi
@Temperature 212 °F
EN min.; EN 10002-5
 630 MPa
@Temperature 50.0 °C
91400 psi
@Temperature 122 °F
EN min.; EN 10002-5
Tensile Strength, Yield  370 MPa
@Strain 0.2 %
53700 psi
@Strain 0.2 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 410 MPa
@Strain 1 %
59500 psi
@Strain 1 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 130 MPa
@Strain 0.2 %,
Temperature 700 °C
18900 psi
@Strain 0.2 %,
Temperature 1290 °F
EN min.
 140 MPa
@Strain 0.2 %,
Temperature 600 °C
20300 psi
@Strain 0.2 %,
Temperature 1110 °F
EN min.; EN 10002-5
 150 MPa
@Strain 0.2 %,
Temperature 500 °C
21800 psi
@Strain 0.2 %,
Temperature 932 °F
EN min.; EN 10002-5
 155 MPa
@Strain 1 %,
Temperature 700 °C
22500 psi
@Strain 1 %,
Temperature 1290 °F
EN min.
 160 MPa
@Strain 0.2 %,
Temperature 400 °C
23200 psi
@Strain 0.2 %,
Temperature 752 °F
EN min.; EN 10002-5
 170 MPa
@Strain 1 %,
Temperature 600 °C
24700 psi
@Strain 1 %,
Temperature 1110 °F
EN min.; EN 10002-5
 170 MPa
@Strain 0.2 %,
Temperature 300 °C
24700 psi
@Strain 0.2 %,
Temperature 572 °F
EN min.; EN 10002-5
 180 MPa
@Strain 1 %,
Temperature 500 °C
26100 psi
@Strain 1 %,
Temperature 932 °F
EN min.; EN 10002-5
 185 MPa
@Strain 0.2 %,
Temperature 200 °C
26800 psi
@Strain 0.2 %,
Temperature 392 °F
EN min.; EN 10002-5
 190 MPa
@Strain 1 %,
Temperature 400 °C
27600 psi
@Strain 1 %,
Temperature 752 °F
EN min.; EN 10002-5
 200 MPa
@Strain 1 %,
Temperature 300 °C
29000 psi
@Strain 1 %,
Temperature 572 °F
EN min.; EN 10002-5
 215 MPa
@Strain 1 %,
Temperature 200 °C
31200 psi
@Strain 1 %,
Temperature 392 °F
EN min.; EN 10002-5
 230 MPa
@Strain 0.2 %,
Temperature 100 °C
33400 psi
@Strain 0.2 %,
Temperature 212 °F
EN min.; EN 10002-5
 265 MPa
@Strain 1 %,
Temperature 100 °C
38400 psi
@Strain 1 %,
Temperature 212 °F
EN min.; EN 10002-5
 280 MPa
@Strain 0.2 %,
Temperature 50.0 °C
40600 psi
@Strain 0.2 %,
Temperature 122 °F
EN min.; EN 10002-5
 315 MPa
@Strain 1 %,
Temperature 50.0 °C
45700 psi
@Strain 1 %,
Temperature 122 °F
EN min.; EN 10002-5
Elongation at Break 50 %50 %Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
Rupture Strength  4.00 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
580 psi
@Temperature 2010 °F,
Time 10000 hour
 7.00 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
1020 psi
@Temperature 1830 °F,
Time 10000 hour
 13.0 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
1890 psi
@Temperature 1650 °F,
Time 10000 hour
 18.0 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
2610 psi
@Temperature 1560 °F,
Time 10000 hour
 27.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
3920 psi
@Temperature 1470 °F,
Time 10000 hour
 41.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
5950 psi
@Temperature 1380 °F,
Time 10000 hour
 63.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
9140 psi
@Temperature 1290 °F,
Time 10000 hour
 98.0 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
14200 psi
@Temperature 1200 °F,
Time 10000 hour
 157 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
22800 psi
@Temperature 1110 °F,
Time 10000 hour
 250 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
36300 psi
@Temperature 1020 °F,
Time 10000 hour
Modulus of Elasticity 200 GPa29000 ksiRT
 120 GPa
@Temperature 1000 °C
17400 ksi
@Temperature 1830 °F
 163 GPa
@Temperature 500 °C
23600 ksi
@Temperature 932 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000840 ohm-cm0.0000840 ohm-cmRT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  18.2 µm/m-°C
@Temperature 500 °C
10.1 µin/in-°F
@Temperature 932 °F
 19.5 µm/m-°C
@Temperature 1000 °C
10.8 µin/in-°F
@Temperature 1830 °F
Specific Heat Capacity 0.500 J/g-°C0.120 BTU/lb-°FRT
 0.580 J/g-°C
@Temperature 500 °C
0.139 BTU/lb-°F
@Temperature 932 °F
Thermal Conductivity 15.0 W/m-K104 BTU-in/hr-ft²-°FRT
 21.2 W/m-K
@Temperature 500 °C
147 BTU-in/hr-ft²-°F
@Temperature 932 °F
 29.0 W/m-K
@Temperature 1000 °C
201 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Maximum Service Temperature, Air 1100 °C2010 °FDry Air
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 900 °C1650 °FStress Relief Annealing (min. 0.5 h)
 1020 - 1120 °C1870 - 2050 °FSolution Annealing
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.090 %0.090 %
Cerium, Ce 1.6 %1.6 %
Chromium, Cr 21 %21 %
Iron, Fe 64.54 %64.54 %
Nickel, Ni 11 %11 %
Nitrogen, N 0.17 %0.17 %
Silicon, Si 1.6 %1.6 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 304H Stainless Steel, Austenitic
310 Stainless Steel, annealed plate
Cast Stainless Steel HK, ACI
Cast Stainless Steel HH, ACI
309 Stainless Steel, annealed, plate

NOUTOK45 / 18760

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.