MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Braskem PCD 0140 HECO Polypropylene Heterophasic Copolymer  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: PCD 0140 is a low melt flow rate heterophasic copolymer with high impact resistance. This resin was developed for steel pipe coating extrusion. PCD 0140 is highly protected against thermal aging and designed for continuous use at high temperatures. Its applications include: undercoating, solid thermal coating, and foam thermal coating.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ASTM-D792
Oxidative Induction Time (OIT) >= 50 min
@Temperature 220 °C
>= 50 min
@Temperature 428 °F
ASTM-D3895
Melt Flow 0.75 g/10 min
@Load 2.16 kg,
Temperature 230 °C
0.75 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM-D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6666ASTM-D2240
Tensile Strength, Yield 25.0 MPa3630 psiASTM-D638
Elongation at Break >= 400 %>= 400 %ASTM-D638
 >= 140 %
@Time 1.26e+7 sec
>= 140 %
@Time 3500 hour
UV Stability; ASTM D155
Elongation at Yield 7.0 %7.0 %ASTM-D638
Flexural Modulus, 1% Secant 1100 MPa160000 psiASTM-D790
Taber Abrasion, mg/1000 Cycles 7.0
@Load 1.00 kg
7.0
@Load 2.20 lb
CS-17; ASTM D4060
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+17 ohm-cm1.00e+17 ohm-cmASTM-D257
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity <= 0.220 W/m-K<= 1.53 BTU-in/hr-ft²-°FASTM C177/C518
Melting Point 163 °C325 °FASTM-D3418
Vicat Softening Point 146 °C
@Load 1.02 kg
295 °F
@Load 2.25 lb
ASTM-D1525

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Braskem PCD 0140BR HECO Polypropylene Heterophasic Copolymer
Braskem PRA 0852 RACO Random Polypropylene Copolymer
Braskem Prisma 3410 RACO Random Polypropylene Copolymer
Diamond, Polycrystalline
Braskem PRB 0131 RACO Random Polypropylene Copolymer

PBRAS940 / 106786

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.