MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ArcelorMittal Complex Phase Steel 600 Very High Strength Cold Rolled Steel
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: Available in the following: uncoated (HCT600C) and electrogalvanized (HCT600C+ZE)

Description: The Complex Phase family of steels supplements ArcelorMittal's VHSS (very high strength steel) product range. These steels are cold formed to make lightweight structural elements. A number of automotive parts, such as sills and door reinforcements, have simple shapes and the steel is therefore only slightly deformed. For this reason, ArcelorMittal has added the Complex Phase family of steels to its range. These steels offer high as-delivered yield strength and good bendability and stretch flangeability.

Applications: Given their high energy absorption capacity and fatigue strength, these grades are particularly well suited for automotive safety components requiring good impact strength and for suspension system components.

Information provided by ArcelorMittal

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 600 - 700 MPa87000 - 102000 psi
Tensile Strength, Yield 360 - 440 MPa52200 - 63800 psi
Elongation at Break >= 19 %>= 19 %L0=80 mm, th<3 mm
Fatigue Strength  <= 495 MPa
@# of Cycles 2.00e+6
<= 71800 psi
@# of Cycles 2.00e+6
 <= 495 MPa
@# of Cycles 1.00e+7
<= 71800 psi
@# of Cycles 1.00e+7
 <= 580 MPa
@# of Cycles 100000
<= 84100 psi
@# of Cycles 100000
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.10 %<= 0.10 %
Iron, Fe >= 97.9 %>= 97.9 %as balance
Manganese, Mn <= 1.6 %<= 1.6 %
Silicon, Si <= 0.40 %<= 0.40 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ArcelorMittal MartINsite® 1200 Cold Rolled Steel
AK Steel 201 Austenitic Stainless steel
ArcelorMittal MartINsite® 1500 Cold Rolled Steel
AISI 1020 Steel, cold rolled
ArcelorMittal HSLA 460 High strength low alloy steel for cold forming, Hot Rolled

NARCE024 / 159932

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.