MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Seals Eastern 7282 Neoprene / Chloroprene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: UL-flame resistant, non-blooming neoprene

Information provided by Seals Eastern, Inc.

Key Words: Polychloroprene Rubber (CR)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.52 g/cc1.52 g/ccASTM D297, 15
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A >= 58>= 58ASTM D2240, Type A
 6262AVG; ASTM D2240, Type A
 73
@Treatment Temp. 100 °C,
Time 605000 sec
73
@Treatment Temp. 212 °F,
Time 168 hour
After Dry Heat Aging; ASTM D865
Tensile Strength at Break >= 11.88 MPa>= 1723 psiASTM D412 Method A
 14.84 MPa2152 psiAVG; ASTM D412 Method A
 12.47 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
1808 psi
@Treatment Temp. 212 °F,
Time 168 hour
After Dry Heat Aging; ASTM D865
Tensile Stress at Strain  1.00 MPa
@Strain 25 %
145 psi
@Strain 25 %
Average; ASTM D412 Method A
 >= 1.03 MPa
@Strain 50 %
>= 149 psi
@Strain 50 %
Minimum; ASTM D412 Method A
 1.49 MPa
@Strain 50 %
216 psi
@Strain 50 %
Average; ASTM D412 Method A
 >= 1.74 MPa
@Strain 100 %
>= 252 psi
@Strain 100 %
Minimum; ASTM D412 Method A
 2.62 MPa
@Strain 100 %
380 psi
@Strain 100 %
Average; ASTM D412 Method A
Elongation at Break >= 287 %>= 287 %ASTM D412 Method A
 362 %362 %AVG; ASTM D412 Method A
 166.5 %
@Treatment Temp. 100 °C,
Time 605000 sec
166.5 %
@Treatment Temp. 212 °F,
Time 168 hour
After Dry Heat Aging; ASTM D865
Modulus of Elasticity 0.00614 GPa0.890 ksiASTM D412 Method A
Poissons Ratio 0.500.50Calculated
Shear Modulus 0.00205 GPa0.297 ksiASTM D412 Method A
Secant Modulus 0.00539 GPa0.782 ksiASTM D412 Method A
Tear Strength Test 198198(psi); ASTM D624, Die B
Compression Set 17 %
@Temperature 100 °C,
Time 252000 sec
17 %
@Temperature 212 °F,
Time 70.0 hour
ASTM D395, Test B
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg -40.0 °C-40.0 °FASTM D1329
 
Descriptive Properties
Strain Energy / Unit Volume at 20% Elongation (psi)16

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Polychloroprene Rubber (CR)
Seals Eastern 5241 Neoprene / Chloroprene
Cos40 Cork/Neoprene Rubber Sheet
Seals Eastern 7065 Neoprene / Chloroprene
Armacell Monarch® F-02001 Neoprene Based Rubber Foam

PSEAL48 / 80195

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.