MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ascend Performance Materials Vydyne® R862H BK0676 Nylon 66, Glass + Mineral Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass/Mineral Filled

Material Notes: Vydyne R862H BK0676 is a general purpose, glass-fiber, mineral-reinforced, heat stabilized PA66 resin. Available in black, this product is also lubricated for improved flow and offers superior surface appearance. R862H BK0676 can be successfully used in a wide range of injection-molding engineering applications. Typical parts include lower cowl top covers, radiator shrouds, fans and mirror brackets, cylinder head covers.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.47 g/cc0.0531 lb/in³DAM; ISO 1183
Moisture Absorption at Equilibrium 1.5 %1.5 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cm
@Thickness 2.00 mm
0.0040 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.011 cm/cm
@Thickness 2.00 mm
0.011 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 98.0 MPa14200 psi50% RH; ISO 527-2
 149 MPa21600 psiDAM; ISO 527-2
Elongation at Break 2.2 %2.2 %50% RH; ISO 527-2
 2.2 %2.2 %DAM; ISO 527-2
Tensile Modulus 7.80 GPa1130 ksi50% RH; ISO 527-2
 10.5 GPa1520 ksiDAM; ISO 527-2
Flexural Strength 120 MPa17400 psi50% RH; ISO 178
 220 MPa31900 psiDAM; ISO 178
Flexural Modulus 5.60 GPa812 ksi50% RH; ISO 178
 10.8 GPa1570 ksiDAM; ISO 178
Poissons Ratio 0.400.40ISO 527-2
Izod Impact, Notched (ISO)  6.00 kJ/m²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
 7.00 kJ/m²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 180/1A
 7.00 kJ/m²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 11.0 kJ/m²
@Temperature 23.0 °C
5.23 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1A
Charpy Impact Unnotched  4.60 J/cm²
@Temperature -30.0 °C
21.9 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eU
 4.80 J/cm²
@Temperature 23.0 °C
22.8 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eU
 4.90 J/cm²
@Temperature 23.0 °C
23.3 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
 5.00 J/cm²
@Temperature -30.0 °C
23.8 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eU
Charpy Impact, Notched  0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 0.600 J/cm²
@Temperature 23.0 °C
2.86 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 18.5 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
10.3 µin/in-°F
@Thickness 0.0787 in,
Temperature 95.0 - 131 °F
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 66.9 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
37.2 µin/in-°F
@Thickness 0.0787 in,
Temperature 73.4 - 131 °F
DAM; ISO 11359-2
Melting Point 260 °C500 °FDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 255 °C491 °FUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 234 °C453 °FUnannealed; DAM; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Middle Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Front Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Nozzle Temperature 280 - 310 °C536 - 590 °FInjection
Melt Temperature 285 - 305 °C545 - 581 °FInjection
Mold Temperature 65.0 - 95.0 °C149 - 203 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 4.00 hour4.00 hourInjection
 
Descriptive Properties
AdditiveHeat Stabilizer
 Lubricant
Agency RatingsASTM, D4066 PA114R40
 ASTM, D6779 PA084R40
AppearanceBlack
Automotive Material SpecificationHYUNDAI MS211-36 Type C
FeaturesCreep Resistant
 Good Dimensional Stability
 Good Flow
 Heat Stabilized
 Lubricated
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ascend Performance Materials Vydyne® R513H NT Nylon 66, 13% Glass Filled
Ascend Performance Materials Vydyne® R513 NT Nylon 66, 13% Glass Filled

PASCE9737 / 220840

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.