MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Tisan TISOPLEN® 30% Glass Fiber Filled Reinforced Heat Stabilized Homopolymer Polypropylene
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 30% Glass Fiber Filler

Material Notes: TISOPLEN has a wide area of application in furniture, durable goods, household appliances, electrics/electronics, and telecommunication industries. General specifications include
  • Low density
  • Low moisture intake
  • High impact resistance
  • Excellent chemical resistance
  • Electrical isolation
  • High performance/affordable price
  • Easy processability
Mineral filled TISOPLEN compounds have a long lasting thermal-dimensional stability, increased mechanical and hardness characteristics, decreased mold shrinkage and improved surface appearance. Glass fiber reinforcement will impart high tensile strength and impact resistance and yield improvements in thermal characteristics of TISOPLEN products. Excellent resistance to weak acids, weak alkalis, and strong alkalis. Good resistance to strong acids and alcohols. Medium resistance to hydrocarbons and engine fuels. Weak resistance to organic solvents.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0397 lb/in³ISO 1183
Moisture Absorption 0.010 %0.010 %ISO 62
Linear Mold Shrinkage 0.0040 cm/cm0.0040 in/in
Ash 30 %30 %ISO 3451
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6969ISO 868
Tensile Strength at Break 95.0 MPa13800 psiISO 527-2
Tensile Strength, Yield 94.0 MPa13600 psiISO 527-2
Elongation at Break 3.0 %3.0 %ISO 527-2
Elongation at Yield 3.0 %3.0 %ISO 527-2
Modulus of Elasticity 5.80 GPa841 ksiISO 527-2
Izod Impact, Notched (ISO) 10.0 kJ/m²4.76 ft-lb/in²ISO 180
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 600 V600 VTS EN 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 165 °C329 °F
Vicat Softening Point 140 °C284 °FISO 306
Heat Distortion Temperature 160 °C320 °FISO 75-2
Flammability, UL94 HBHB
 
Processing PropertiesMetricEnglishComments
Feed Temperature 70.0 °C158 °F
Rear Barrel Temperature 190 - 210 °C374 - 410 °FAft-1. Region Temperature
Middle Barrel Temperature 190 - 210 °C374 - 410 °FMid-2. Region Temperature
Front Barrel Temperature 190 - 210 °C374 - 410 °FPre-3. Region Temperature
Nozzle Temperature 200 °C392 °F
Melt Temperature 170 - 190 °C338 - 374 °F
Drying Temperature 80.0 °C176 °FPredrying Temperature
Dry Time 1 hour1 hourPredrying Time
 
Descriptive Properties
Block Temperature45°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tisan TISESTER® UNR Polybutylene Terephthalate
Tisan TISLAMID® 6 UNR Nylon 6
Overview of materials for Polypropylene Copolymer
Overview of materials for Polypropylene, Flame Retardant
Tisan TISAKRIL® 30% Glass Fiber Reinforced ABS

PTIS031 / 79466

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.