Lubrizol ESTALOC® 59300 Polyester-Type, Reinforced Engineering Thermoplastic Polyurethane
Categories:
Polymer
;
Thermoplastic
;
Elastomer, TPE
;
Polyurethane, TP
;
Thermoplastic Polyurethane, Elastomer, Glass Filled
Material Notes:
Features:
Fast Cycling, Dimensional Stability, Durability, Aesthetics, Low Temperature Impact
Uses:
Injection Molding
Availability: Americas, Europe, Middle East, Africa, India and Asia
Information provided by Lubrizol
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.45
g/cc
1.45
g/cc
ASTM D792
Filler Content
30 %
30 %
Glass Fiber
Maximum Moisture Content
0.020
0.020
Linear Mold Shrinkage
0.00040
cm/cm
0.00040
in/in
flex bar; ASTM D955
0.0010
cm/cm
0.0010
in/in
average flow and against flow, disc; ASTM D955
Mechanical Properties
Metric
English
Comments
Hardness, Shore D
72 - 78
@Time 5.00 sec
72 - 78
@Time 0.00139 hour
ASTM D2240
Tensile Strength
83.0
MPa
12000
psi
ASTM D638
Elongation at Break
20 %
20 %
ASTM D638
Tensile Modulus
3.65
GPa
530
ksi
ASTM D638
Flexural Strength
90.0
MPa
13100
psi
ASTM D790
Flexural Modulus
2.90
GPa
420
ksi
ASTM D790
Izod Impact, Notched
4.27
J/cm
8.00
ft-lb/in
ASTM D256
1.28
J/cm
@Temperature -40.0 °C
2.40
ft-lb/in
@Temperature -40.0 °F
ASTM D256
Processing Properties
Metric
English
Comments
Rear Barrel Temperature
210
°C
410
°F
Middle Barrel Temperature
221
°C
430
°F
Front Barrel Temperature
224
°C
435
°F
Nozzle Temperature
232
°C
450
°F
Melt Temperature
232
°C
450
°F
Drying Temperature
104
°C
219
°F
Dry Time
2.00
-
4.00
hour
2.00
-
4.00
hour
Dew Point
-40.0
°C
-40.0
°F
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Lubrizol ESTALOC® 59600 Polyester-Type, Reinforced Engineering Thermoplastic Polyurethane
Lubrizol ESTALOC® 59200 Ester-Type, Reinforced Engineering Thermoplastic
Lubrizol ESTALOC® 59010 Polyester-Type, Reinforced Engineering Thermoplastic Polyurethane
Lubrizol ESTALOC® 59104 Ester-Type, Reinforced Engineering Thermoplastic
Kingfa JH960 HT10 Non-halogenated Flame Retardant PC/ABS Alloy
PNOVEON004 / 55269
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.