Physical Properties | Metric | English | Comments |
---|
Density | 3.65 g/cc | 0.132 lb/in³ |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 52.3 | 52.3 |
Alkali Class, AR | 3.3 | 3.3 |
Stain Resistance Class, FR | 1.0 | 1.0 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 372 | 372 |
Modulus of Elasticity | 70.0 GPa | 10200 ksi |
Poissons Ratio | 0.30 | 0.30 |
Shear Modulus | 26.9 GPa | 3900 ksi |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 13.7 µm/m-°C @Temperature -30.0 - 70.0 °C | 7.61 µin/in-°F @Temperature -22.0 - 158 °F |
| 15.7 µm/m-°C @Temperature 20.0 - 300 °C | 8.72 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.710 J/g-°C | 0.170 BTU/lb-°F |
Thermal Conductivity | 0.760 W/m-K | 5.27 BTU-in/hr-ft²-°F |
Transformation Temperature, Tg | 445 °C | 833 °F |
Softening Point | 508 °C | 946 °F |
Annealing Point | 448 °C | 838 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.441 @Wavelength 232.4 nm | 1.441 @Wavelength 232.4 nm |
| 1.443 @Wavelength 1970.1 nm | 1.443 @Wavelength 1970.1 nm |
| 1.446 @Wavelength 1529.6 nm | 1.446 @Wavelength 1529.6 nm |
| 1.449 @Wavelength 1060 nm | 1.449 @Wavelength 1060 nm |
| 1.45 @Wavelength 1014 nm | 1.45 @Wavelength 1014 nm |
| 1.451 @Wavelength 852.1 nm | 1.451 @Wavelength 852.1 nm |
| 1.453 @Wavelength 706.5 nm | 1.453 @Wavelength 706.5 nm |
| 1.454 @Wavelength 656.3 nm | 1.454 @Wavelength 656.3 nm |
| 1.454 @Wavelength 632.8 nm | 1.454 @Wavelength 632.8 nm |
| 1.454 @Wavelength 643.8 nm | 1.454 @Wavelength 643.8 nm |
| 1.455 @Wavelength 589.3 nm | 1.455 @Wavelength 589.3 nm |
| 1.456 @Wavelength 587.6 nm | 1.456 @Wavelength 587.6 nm |
| 1.459 @Wavelength 486.1 nm | 1.459 @Wavelength 486.1 nm |
| 1.459 @Wavelength 480 nm | 1.459 @Wavelength 480 nm |
| 1.462 @Wavelength 435.8 nm | 1.462 @Wavelength 435.8 nm |
| 1.464 @Wavelength 404.7 nm | 1.464 @Wavelength 404.7 nm |
| 1.468 @Wavelength 365 nm | 1.468 @Wavelength 365 nm |
| 1.471 @Wavelength 334.1 nm | 1.471 @Wavelength 334.1 nm |
| 1.475 @Wavelength 546.1 nm | 1.475 @Wavelength 546.1 nm |
Abbe Number | 90.47 | 90.47 |
| 90.9 | 90.9 |
Optical Dispersion | 0.005017 | 0.005017 |
| 0.005053 | 0.005053 |
Transmission, Visible | 99.1 % @Thickness 25.0 mm, Wavelength 420 nm | 99.1 % @Thickness 0.984 in, Wavelength 420 nm |
| 99.1 % @Thickness 25.0 mm, Wavelength 436 nm | 99.1 % @Thickness 0.984 in, Wavelength 436 nm |
| 99.2 % @Thickness 25.0 mm, Wavelength 460 nm | 99.2 % @Thickness 0.984 in, Wavelength 460 nm |
| 99.3 % @Thickness 25.0 mm, Wavelength 660 nm | 99.3 % @Thickness 0.984 in, Wavelength 660 nm |
| 99.3 % @Thickness 25.0 mm, Wavelength 700 nm | 99.3 % @Thickness 0.984 in, Wavelength 700 nm |
| 99.4 % @Thickness 25.0 mm, Wavelength 500 nm | 99.4 % @Thickness 0.984 in, Wavelength 500 nm |
| 99.4 % @Thickness 25.0 mm, Wavelength 580 nm | 99.4 % @Thickness 0.984 in, Wavelength 580 nm |
| 99.4 % @Thickness 25.0 mm, Wavelength 620 nm | 99.4 % @Thickness 0.984 in, Wavelength 620 nm |
| 99.5 % @Thickness 25.0 mm, Wavelength 546 nm | 99.5 % @Thickness 0.984 in, Wavelength 546 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 436 nm | 99.6 % @Thickness 0.394 in, Wavelength 436 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 420 nm | 99.6 % @Thickness 0.394 in, Wavelength 420 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 620 nm | 99.7 % @Thickness 0.394 in, Wavelength 620 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 660 nm | 99.7 % @Thickness 0.394 in, Wavelength 660 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 700 nm | 99.7 % @Thickness 0.394 in, Wavelength 700 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 500 nm | 99.8 % @Thickness 0.394 in, Wavelength 500 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 580 nm | 99.8 % @Thickness 0.394 in, Wavelength 580 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 546 nm | 99.8 % @Thickness 0.394 in, Wavelength 546 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 460 nm | 99.8 % @Thickness 0.394 in, Wavelength 460 nm |
IR Transmittance | 99.3 % @Thickness 25.0 mm, Wavelength 2500 nm | 99.3 % @Thickness 0.984 in, Wavelength 2500 nm |
| 99.5 % @Thickness 25.0 mm, Wavelength 1060 nm | 99.5 % @Thickness 0.984 in, Wavelength 1060 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 2325 nm | 99.6 % @Thickness 0.984 in, Wavelength 2325 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 2500 nm | 99.7 % @Thickness 0.394 in, Wavelength 2500 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 2325 nm | 99.8 % @Thickness 0.394 in, Wavelength 2325 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1060 nm | 99.8 % @Thickness 0.394 in, Wavelength 1060 nm |
| 99.8 % @Thickness 25.0 mm, Wavelength 1530 nm | 99.8 % @Thickness 0.984 in, Wavelength 1530 nm |
| 99.8 % @Thickness 25.0 mm, Wavelength 1970 nm | 99.8 % @Thickness 0.984 in, Wavelength 1970 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1970 nm | 99.9 % @Thickness 0.394 in, Wavelength 1970 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1530 nm | 99.9 % @Thickness 0.394 in, Wavelength 1530 nm |
UV Transmittance | 0.50 % @Thickness 25.0 mm, Wavelength 260 nm | 0.50 % @Thickness 0.984 in, Wavelength 260 nm |
| 1.0 % @Thickness 25.0 mm, Wavelength 270 nm | 1.0 % @Thickness 0.984 in, Wavelength 270 nm |
| 2.8 % @Thickness 25.0 mm, Wavelength 280 nm | 2.8 % @Thickness 0.984 in, Wavelength 280 nm |
| 8.0 % @Thickness 25.0 mm, Wavelength 290 nm | 8.0 % @Thickness 0.984 in, Wavelength 290 nm |
| 9.0 % @Thickness 10.0 mm, Wavelength 250 nm | 9.0 % @Thickness 0.394 in, Wavelength 250 nm |
| 10.9 % @Thickness 10.0 mm, Wavelength 260 nm | 10.9 % @Thickness 0.394 in, Wavelength 260 nm |
| 15.2 % @Thickness 10.0 mm, Wavelength 270 nm | 15.2 % @Thickness 0.394 in, Wavelength 270 nm |
| 20 % @Thickness 25.0 mm, Wavelength 300 nm | 20 % @Thickness 0.984 in, Wavelength 300 nm |
| 23.9 % @Thickness 10.0 mm, Wavelength 280 nm | 23.9 % @Thickness 0.394 in, Wavelength 280 nm |
| 36.4 % @Thickness 10.0 mm, Wavelength 290 nm | 36.4 % @Thickness 0.394 in, Wavelength 290 nm |
| 40 % @Thickness 25.0 mm, Wavelength 310 nm | 40 % @Thickness 0.984 in, Wavelength 310 nm |
| 52.5 % @Thickness 10.0 mm, Wavelength 300 nm | 52.5 % @Thickness 0.394 in, Wavelength 300 nm |
| 61 % @Thickness 25.0 mm, Wavelength 320 nm | 61 % @Thickness 0.984 in, Wavelength 320 nm |
| 69.3 % @Thickness 10.0 mm, Wavelength 310 nm | 69.3 % @Thickness 0.394 in, Wavelength 310 nm |
| 82.1 % @Thickness 10.0 mm, Wavelength 320 nm | 82.1 % @Thickness 0.394 in, Wavelength 320 nm |
| 83 % @Thickness 25.0 mm, Wavelength 334 nm | 83 % @Thickness 0.984 in, Wavelength 334 nm |
| 92.8 % @Thickness 10.0 mm, Wavelength 334 nm | 92.8 % @Thickness 0.394 in, Wavelength 334 nm |
| 94 % @Thickness 25.0 mm, Wavelength 350 nm | 94 % @Thickness 0.984 in, Wavelength 350 nm |
| 97.5 % @Thickness 25.0 mm, Wavelength 365 nm | 97.5 % @Thickness 0.984 in, Wavelength 365 nm |
| 97.6 % @Thickness 10.0 mm, Wavelength 350 nm | 97.6 % @Thickness 0.394 in, Wavelength 350 nm |
| 98 % @Thickness 25.0 mm, Wavelength 370 nm | 98 % @Thickness 0.984 in, Wavelength 370 nm |
| 98.7 % @Thickness 25.0 mm, Wavelength 380 nm | 98.7 % @Thickness 0.984 in, Wavelength 380 nm |
| 99 % @Thickness 25.0 mm, Wavelength 390 nm | 99 % @Thickness 0.984 in, Wavelength 390 nm |
| 99 % @Thickness 10.0 mm, Wavelength 365 nm | 99 % @Thickness 0.394 in, Wavelength 365 nm |
| 99.1 % @Thickness 25.0 mm, Wavelength 405 nm | 99.1 % @Thickness 0.984 in, Wavelength 405 nm |
| 99.1 % @Thickness 25.0 mm, Wavelength 400 nm | 99.1 % @Thickness 0.984 in, Wavelength 400 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 370 nm | 99.2 % @Thickness 0.394 in, Wavelength 370 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 380 nm | 99.5 % @Thickness 0.394 in, Wavelength 380 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 400 nm | 99.6 % @Thickness 0.394 in, Wavelength 400 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 390 nm | 99.6 % @Thickness 0.394 in, Wavelength 390 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 405 nm | 99.6 % @Thickness 0.394 in, Wavelength 405 nm |
|
Descriptive Properties |
---|
Acid resistance class | 4 |
Climatic resistance | 1 |
Phosphate resistance | 4.3 |
Stress optical coefficient | 0.54 |
Water resistance class | 1 |
Yield point/sag temperature | 475°C |