MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 5154-H112
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition information provided by the Aluminum Association and is not for design.

Key Words: ISO AlMg3.5; Aluminium 5154-H112; AA5154-H112; UNS A95154; Al5154-H112
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.66 g/cc0.0961 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 6363AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 8686Converted from Brinell Hardness Value
Hardness, Vickers 7373Converted from Brinell Hardness Value
Tensile Strength, Ultimate 241 MPa35000 psiAA; Typical
 >= 205 MPa
@Thickness 1.27 - 76.2 mm
>= 29700 psi
@Thickness 0.0500 - 3.00 in
 >= 220 MPa
@Thickness 6.35 - 12.7 mm
>= 31900 psi
@Thickness 0.250 - 0.499 in
Tensile Strength, Yield 117 MPa17000 psiAA; Typical
 >= 75.0 MPa
@Thickness 1.27 - 76.2 mm
>= 10900 psi
@Thickness 0.0500 - 3.00 in
 >= 125 MPa
@Thickness 6.35 - 12.7 mm
>= 18100 psi
@Thickness 0.250 - 0.499 in
Elongation at Break  >= 8.0 %
@Thickness 6.35 - 12.7 mm
>= 8.0 %
@Thickness 0.250 - 0.499 in
 11 - 15 %
@Thickness 1.27 - 76.2 mm
11 - 15 %
@Thickness 0.0500 - 3.00 in
 25 %
@Thickness 1.59 mm
25 %
@Thickness 0.0625 in
AA; Typical
Modulus of Elasticity 70.3 GPa10200 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33
Fatigue Strength 117 MPa
@# of Cycles 5.00e+8
17000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 25.9 GPa3760 ksi
Shear Strength 145 MPa21000 psiCalculated value.
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000532 ohm-cm
@Temperature 20.0 °C
0.00000532 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  22.1 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.3 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.9 µm/m-°C
@Temperature 20.0 - 100 °C
13.3 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 24.9 µm/m-°C
@Temperature 20.0 - 200 °C
13.8 µin/in-°F
@Temperature 68.0 - 392 °F
 25.9 µm/m-°C
@Temperature 20.0 - 300 °C
14.4 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.900 J/g-°C0.215 BTU/lb-°F
Thermal Conductivity 125 W/m-K870 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 593 - 643 °C1100 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 593 °C1100 °FAA; Typical
Liquidus 643 °C1190 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 343 °C650 °Fholding at temperature not required
Hot-Working Temperature 260 - 510 °C500 - 950 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 94.3 - 96.8 %94.3 - 96.8 %As remainder
Beryllium, Be <= 0.0008 %<= 0.0008 %welding electrode and filler wire only
Chromium, Cr 0.15 - 0.35 %0.15 - 0.35 %
Copper, Cu <= 0.10 %<= 0.10 %
Iron, Fe <= 0.40 %<= 0.40 %
Magnesium, Mg 3.1 - 3.9 %3.1 - 3.9 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.25 %<= 0.25 %
Titanium, Ti <= 0.20 %<= 0.20 %
Zinc, Zn <= 0.20 %<= 0.20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 5154-O
Aluminum 5154-H32
AISI 4140 Steel, annealed at 815°C (1500°F) furnace cooled 11°C (20°F)/hour to 665°C (1230°F), air cooled, 25 mm (1 in.) round
Aluminum 5154-H36
Aluminum 5154-H34

MA5154H112 / 9210

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.