Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.47 g/cc | 1.47 g/cc |
Density | 1.45 g/cc | 0.0524 lb/in³ |
Filler Content | 35 % | 35 % |
Linear Mold Shrinkage | 0.010 cm/cm @Thickness 1.60 mm | 0.010 in/in @Thickness 0.0630 in |
| 0.010 cm/cm @Thickness 3.20 mm | 0.010 in/in @Thickness 0.126 in |
Linear Mold Shrinkage, Flow | 0.0020 cm/cm @Thickness 2.00 mm | 0.0020 in/in @Thickness 0.0787 in |
| 0.0025 cm/cm @Thickness 1.60 mm | 0.0025 in/in @Thickness 0.0630 in |
| 0.0030 cm/cm @Thickness 3.20 mm | 0.0030 in/in @Thickness 0.126 in |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell M | 105 | 105 |
Hardness, Rockwell R | 124 | 124 |
Tensile Strength at Break | 180 MPa @Temperature 23.0 °C | 26100 psi @Temperature 73.4 °F |
| 200 MPa @Temperature 23.0 °C | 29000 psi @Temperature 73.4 °F |
Tensile Strength | 72.4 MPa @Temperature 200 °C | 10500 psi @Temperature 392 °F |
| 80.0 MPa @Temperature 175 °C | 11600 psi @Temperature 347 °F |
| 89.0 MPa @Temperature 150 °C | 12900 psi @Temperature 302 °F |
| 124 MPa @Temperature 100 °C | 18000 psi @Temperature 212 °F |
| 168 MPa @Temperature 23.0 °C | 24400 psi @Temperature 73.4 °F |
| 188 MPa @Temperature 60.0 °C | 27300 psi @Temperature 140 °F |
| 204 MPa @Temperature 23.0 °C | 29600 psi @Temperature 73.4 °F |
| 230 MPa @Temperature -40.0 °C | 33400 psi @Temperature -40.0 °F |
Elongation at Break | 2.1 % @Temperature 23.0 °C | 2.1 % @Temperature 73.4 °F |
| 2.3 % @Temperature -40.0 °C | 2.3 % @Temperature -40.0 °F |
| 2.3 % @Temperature 23.0 °C | 2.3 % @Temperature 73.4 °F |
| 2.7 % @Temperature 23.0 °C | 2.7 % @Temperature 73.4 °F |
| 2.8 % @Temperature 60.0 °C | 2.8 % @Temperature 140 °F |
| 3.3 % @Temperature 23.0 °C | 3.3 % @Temperature 73.4 °F |
| 4.5 % @Temperature 100 °C | 4.5 % @Temperature 212 °F |
| 5.4 % @Temperature 200 °C | 5.4 % @Temperature 392 °F |
| 5.5 % @Temperature 150 °C | 5.5 % @Temperature 302 °F |
| 5.5 % @Temperature 175 °C | 5.5 % @Temperature 347 °F |
Tensile Modulus | 4.40 GPa @Temperature 200 °C | 638 ksi @Temperature 392 °F |
| 4.80 GPa @Temperature 175 °C | 696 ksi @Temperature 347 °F |
| 5.20 GPa @Temperature 150 °C | 754 ksi @Temperature 302 °F |
| 7.30 GPa @Temperature 100 °C | 1060 ksi @Temperature 212 °F |
| 10.3 GPa @Temperature 23.0 °C | 1490 ksi @Temperature 73.4 °F |
| 11.2 GPa @Temperature 60.0 °C | 1620 ksi @Temperature 140 °F |
| 11.7 GPa @Temperature -40.0 °C | 1700 ksi @Temperature -40.0 °F |
| 11.7 GPa @Temperature 23.0 °C | 1700 ksi @Temperature 73.4 °F |
| 12.0 GPa @Temperature 23.0 °C | 1740 ksi @Temperature 73.4 °F |
| 12.5 GPa @Temperature 23.0 °C | 1810 ksi @Temperature 73.4 °F |
Flexural Strength | 249 MPa @Temperature 23.0 °C | 36100 psi @Temperature 73.4 °F |
| 261 MPa @Temperature 60.0 °C | 37900 psi @Temperature 140 °F |
| 299 MPa @Temperature 23.0 °C | 43400 psi @Temperature 73.4 °F |
| 352 MPa @Temperature -40.0 °C | 51100 psi @Temperature -40.0 °F |
| 96.0 MPa @Strain 5.0 %, Temperature 200 °C | 13900 psi @Strain 5.0 %, Temperature 392 °F |
| 114 MPa @Strain 5.0 %, Temperature 175 °C | 16500 psi @Strain 5.0 %, Temperature 347 °F |
| 128 MPa @Strain 5.0 %, Temperature 150 °C | 18600 psi @Strain 5.0 %, Temperature 302 °F |
| 181 MPa @Strain 5.0 %, Temperature 100 °C | 26300 psi @Strain 5.0 %, Temperature 212 °F |
Flexural Modulus | 3.46 GPa @Temperature 200 °C | 502 ksi @Temperature 392 °F |
| 3.63 GPa @Temperature 175 °C | 526 ksi @Temperature 347 °F |
| 3.81 GPa @Temperature 150 °C | 553 ksi @Temperature 302 °F |
| 5.09 GPa @Temperature 100 °C | 738 ksi @Temperature 212 °F |
| 8.30 GPa @Temperature 23.0 °C | 1200 ksi @Temperature 73.4 °F |
| 9.19 GPa @Temperature 60.0 °C | 1330 ksi @Temperature 140 °F |
| 10.19 GPa @Temperature 23.0 °C | 1478 ksi @Temperature 73.4 °F |
| 10.62 GPa @Temperature -40.0 °C | 1540 ksi @Temperature -40.0 °F |
Compressive Strength | 71.0 MPa @Temperature 200 °C | 10300 psi @Temperature 392 °F |
| 89.0 MPa @Temperature 175 °C | 12900 psi @Temperature 347 °F |
| 102 MPa @Temperature 150 °C | 14800 psi @Temperature 302 °F |
| 166 MPa @Temperature 100 °C | 24100 psi @Temperature 212 °F |
| 245 MPa @Temperature 60.0 °C | 35500 psi @Temperature 140 °F |
| 281 MPa @Temperature 23.0 °C | 40800 psi @Temperature 73.4 °F |
| 355 MPa @Temperature -40.0 °C | 51500 psi @Temperature -40.0 °F |
Shear Strength | 79.3 MPa @Temperature 23.0 °C | 11500 psi @Temperature 73.4 °F |
| 91.7 MPa @Temperature 23.0 °C | 13300 psi @Temperature 73.4 °F |
Izod Impact, Notched | 0.910 J/cm @Temperature -40.0 °C | 1.70 ft-lb/in @Temperature -40.0 °F |
| 0.910 J/cm @Temperature -40.0 °C | 1.70 ft-lb/in @Temperature -40.0 °F |
| 0.910 J/cm @Temperature 23.0 °C | 1.70 ft-lb/in @Temperature 73.4 °F |
| 0.910 J/cm @Temperature 23.0 °C | 1.70 ft-lb/in @Temperature 73.4 °F |
Izod Impact, Unnotched | 8.50 J/cm @Temperature 23.0 °C | 15.9 ft-lb/in @Temperature 73.4 °F |
| 10.1 J/cm @Temperature 23.0 °C | 18.9 ft-lb/in @Temperature 73.4 °F |
Izod Impact, Unnotched (ISO) | 40.0 kJ/m² @Temperature 23.0 °C | 19.0 ft-lb/in² @Temperature 73.4 °F |
| 45.0 kJ/m² @Temperature 23.0 °C | 21.4 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact Unnotched | 3.50 J/cm² @Temperature -30.0 °C | 16.7 ft-lb/in² @Temperature -22.0 °F |
| 4.00 J/cm² @Temperature -30.0 °C | 19.0 ft-lb/in² @Temperature -22.0 °F |
| 4.00 J/cm² @Temperature 23.0 °C | 19.0 ft-lb/in² @Temperature 73.4 °F |
| 4.50 J/cm² @Temperature 23.0 °C | 21.4 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact, Notched | 0.600 J/cm² @Temperature -30.0 °C | 2.86 ft-lb/in² @Temperature -22.0 °F |
| 0.700 J/cm² @Temperature -30.0 °C | 3.33 ft-lb/in² @Temperature -22.0 °F |
| 0.900 J/cm² @Temperature 23.0 °C | 4.28 ft-lb/in² @Temperature 73.4 °F |
| 0.950 J/cm² @Temperature 23.0 °C | 4.52 ft-lb/in² @Temperature 73.4 °F |
Tensile Creep Modulus, 1 hour | 10000 MPa @Temperature 23.0 °C | 1.45e+6 psi @Temperature 73.4 °F |
Tensile Creep Modulus, 1000 hours | 8500 MPa @Temperature 23.0 °C | 1.23e+6 psi @Temperature 73.4 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+15 ohm-cm @Temperature 23.0 °C | 1.00e+15 ohm-cm @Temperature 73.4 °F |
| 1.00e+15 ohm-cm @Temperature 23.0 °C | 1.00e+15 ohm-cm @Temperature 73.4 °F |
Surface Resistance | 1.00e+15 ohm @Temperature 23.0 °C | 1.00e+15 ohm @Temperature 73.4 °F |
| 1.00e+15 ohm @Temperature 23.0 °C | 1.00e+15 ohm @Temperature 73.4 °F |
Dielectric Constant | 3.8 @Frequency 1e+6 Hz, Temperature 23.0 °C | 3.8 @Frequency 1e+6 Hz, Temperature 73.4 °F |
| 3.9 @Frequency 1000 Hz, Temperature 23.0 °C | 3.9 @Frequency 1000 Hz, Temperature 73.4 °F |
| 4.2 @Frequency 1e+6 Hz, Temperature 60.0 °C | 4.2 @Frequency 1e+6 Hz, Temperature 140 °F |
| 4.4 @Frequency 1000 Hz, Temperature 60.0 °C | 4.4 @Frequency 1000 Hz, Temperature 140 °F |
| 4.7 @Frequency 1e+6 Hz, Temperature 100 °C | 4.7 @Frequency 1e+6 Hz, Temperature 212 °F |
| 5.6 @Frequency 1000 Hz, Temperature 100 °C | 5.6 @Frequency 1000 Hz, Temperature 212 °F |
| 7.9 @Frequency 1e+6 Hz, Temperature 150 °C | 7.9 @Frequency 1e+6 Hz, Temperature 302 °F |
| 9.9 @Frequency 1e+6 Hz, Temperature 175 °C | 9.9 @Frequency 1e+6 Hz, Temperature 347 °F |
| 12 @Frequency 1e+6 Hz, Temperature 200 °C | 12 @Frequency 1e+6 Hz, Temperature 392 °F |
| 35 @Frequency 1000 Hz, Temperature 150 °C | 35 @Frequency 1000 Hz, Temperature 302 °F |
| 85 @Frequency 1000 Hz, Temperature 175 °C | 85 @Frequency 1000 Hz, Temperature 347 °F |
| 136 @Frequency 1000 Hz, Temperature 200 °C | 136 @Frequency 1000 Hz, Temperature 392 °F |
Dielectric Strength | 0.800 kV/mm @Temperature 200 °C | 20.3 kV/in @Temperature 392 °F |
| 1.20 kV/mm @Temperature 175 °C | 30.5 kV/in @Temperature 347 °F |
| 1.90 kV/mm @Temperature 150 °C | 48.3 kV/in @Temperature 302 °F |
| 16.4 kV/mm @Temperature 100 °C | 417 kV/in @Temperature 212 °F |
| 27.5 kV/mm @Temperature 60.0 °C | 699 kV/in @Temperature 140 °F |
| 27.5 kV/mm @Thickness 3.20 mm, Temperature 23.0 °C | 699 kV/in @Thickness 0.126 in, Temperature 73.4 °F |
Dissipation Factor | 0.010 @Frequency 1000 Hz, Temperature 23.0 °C | 0.010 @Frequency 1000 Hz, Temperature 73.4 °F |
| 0.010 @Frequency 1000 Hz, Temperature 60.0 °C | 0.010 @Frequency 1000 Hz, Temperature 140 °F |
| 0.010 @Frequency 1e+6 Hz, Temperature 23.0 °C | 0.010 @Frequency 1e+6 Hz, Temperature 73.4 °F |
| 0.010 @Frequency 1e+6 Hz, Temperature 60.0 °C | 0.010 @Frequency 1e+6 Hz, Temperature 140 °F |
| 0.040 @Frequency 1e+6 Hz, Temperature 100 °C | 0.040 @Frequency 1e+6 Hz, Temperature 212 °F |
| 0.10 @Frequency 1000 Hz, Temperature 100 °C | 0.10 @Frequency 1000 Hz, Temperature 212 °F |
| 0.15 @Frequency 1e+6 Hz, Temperature 150 °C | 0.15 @Frequency 1e+6 Hz, Temperature 302 °F |
| 0.19 @Frequency 1e+6 Hz, Temperature 175 °C | 0.19 @Frequency 1e+6 Hz, Temperature 347 °F |
| 0.39 @Frequency 1e+6 Hz, Temperature 200 °C | 0.39 @Frequency 1e+6 Hz, Temperature 392 °F |
| 0.75 @Frequency 1000 Hz, Temperature 150 °C | 0.75 @Frequency 1000 Hz, Temperature 302 °F |
| 0.85 @Frequency 1000 Hz, Temperature 175 °C | 0.85 @Frequency 1000 Hz, Temperature 347 °F |
Comparative Tracking Index | 600 V @Temperature 23.0 °C | 600 V @Temperature 73.4 °F |
| 600 V @Temperature 23.0 °C | 600 V @Temperature 73.4 °F |
| >= 600 V @Temperature 23.0 °C | >= 600 V @Temperature 73.4 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 13.0 µm/m-°C @Temperature 125 - 200 °C | 7.22 µin/in-°F @Temperature 257 - 392 °F |
| 13.0 µm/m-°C @Temperature 125 - 200 °C | 7.22 µin/in-°F @Temperature 257 - 392 °F |
| 15.0 µm/m-°C @Temperature 55.0 - 125 °C | 8.33 µin/in-°F @Temperature 131 - 257 °F |
| 15.0 µm/m-°C @Temperature 55.0 - 125 °C | 8.33 µin/in-°F @Temperature 131 - 257 °F |
| 20.0 µm/m-°C @Temperature -40.0 - 23.0 °C | 11.1 µin/in-°F @Temperature -40.0 - 73.4 °F |
| 20.0 µm/m-°C @Temperature -40.0 - 23.0 °C | 11.1 µin/in-°F @Temperature -40.0 - 73.4 °F |
| 21.0 µm/m-°C @Temperature 23.0 - 55.0 °C | 11.7 µin/in-°F @Temperature 73.4 - 131 °F |
| 21.0 µm/m-°C @Temperature 23.0 - 55.0 °C | 11.7 µin/in-°F @Temperature 73.4 - 131 °F |
CTE, linear, Transverse to Flow | 57.0 µm/m-°C @Temperature -40.0 - 23.0 °C | 31.7 µin/in-°F @Temperature -40.0 - 73.4 °F |
| 57.0 µm/m-°C @Temperature -40.0 - 23.0 °C | 31.7 µin/in-°F @Temperature -40.0 - 73.4 °F |
| 62.0 µm/m-°C @Temperature 23.0 - 55.0 °C | 34.4 µin/in-°F @Temperature 73.4 - 131 °F |
| 62.0 µm/m-°C @Temperature 23.0 - 55.0 °C | 34.4 µin/in-°F @Temperature 73.4 - 131 °F |
| 77.0 µm/m-°C @Temperature 55.0 - 125 °C | 42.8 µin/in-°F @Temperature 131 - 257 °F |
| 77.0 µm/m-°C @Temperature 55.0 - 125 °C | 42.8 µin/in-°F @Temperature 131 - 257 °F |
| 95.0 µm/m-°C @Temperature 125 - 200 °C | 52.8 µin/in-°F @Temperature 257 - 392 °F |
| 95.0 µm/m-°C @Temperature 125 - 200 °C | 52.8 µin/in-°F @Temperature 257 - 392 °F |
Melting Point | 305 °C | 581 °F |
| 310 °C | 590 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 285 °C | 545 °F |
| 288 °C | 550 °F |
UL RTI, Electrical | 150 °C @Thickness 0.750 mm | 302 °F @Thickness 0.0295 in |
| 150 °C @Thickness 3.00 mm | 302 °F @Thickness 0.118 in |
| 150 °C @Thickness 1.50 mm | 302 °F @Thickness 0.0591 in |
UL RTI, Mechanical with Impact | 125 °C @Thickness 3.00 mm | 257 °F @Thickness 0.118 in |
| 125 °C @Thickness 1.50 mm | 257 °F @Thickness 0.0591 in |
| 125 °C @Thickness 0.750 mm | 257 °F @Thickness 0.0295 in |
UL RTI, Mechanical without Impact | 130 °C @Thickness 0.750 mm | 266 °F @Thickness 0.0295 in |
| 140 °C @Thickness 1.50 mm | 284 °F @Thickness 0.0591 in |
| 150 °C @Thickness 3.00 mm | 302 °F @Thickness 0.118 in |
Flammability, UL94 | HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 0.850 mm | HB @Thickness 0.0335 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
| HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
Oxygen Index | 25 % | 25 % |
| 25 % | 25 % |
Glow Wire Ignition Temperature | 725 °C @Thickness 1.50 mm | 1340 °F @Thickness 0.0591 in |
| 775 °C @Thickness 0.750 mm | 1430 °F @Thickness 0.0295 in |
| 775 °C @Thickness 3.00 mm | 1430 °F @Thickness 0.118 in |
Glow Wire Flammability Index | 700 °C @Thickness 1.50 mm | 1290 °F @Thickness 0.0591 in |
| 750 °C @Thickness 0.750 mm | 1380 °F @Thickness 0.0295 in |
| 850 °C @Thickness 3.00 mm | 1560 °F @Thickness 0.118 in |
|
Processing Properties | Metric | English | Comments |
---|
Melt Temperature | 325 °C | 617 °F |
| 320 - 330 °C | 608 - 626 °F |
Mold Temperature | 95.0 °C | 203 °F |
| 85.0 - 105 °C | 185 - 221 °F |
Drying Temperature | 100 °C | 212 °F |
Dry Time | 6.00 - 8.00 hour | 6.00 - 8.00 hour |
Moisture Content | <= 0.10 % | <= 0.10 % |
|
Descriptive Properties |
---|
Additive | Heat Stabilizer |
| Lubricant |
Appearance | Natural Color |
Drying Recommended | Yes, if moisture content of resin exceeds recommended level |
Features | Heat Aging Resistance, Good |
Filler | Glass fiber reinforcement |
Forms | Pellets |
Generic | Polyphthalamide (PPA) |
Heat Stabilized | Yes |
Material Status | Preliminary Data |
Part Marking Code | >PA6T/66-GF35< |
| >PPA-GF35< |
Polymer Family | High performance polyamide |
Polymer Type | Partially Aromatic PA, PPA |
Processing Method | Injection Molding |
Product Category | Glass Reinforced Resins |
Region Available - Global | Yes |
Resin Identification | PA6T/66-GF35 |
Ultrasonic Weldable | Yes |
Uses | Automotive Applications |