MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 6063-T835
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Applications include pipe, railings, furniture, architectural extrusions, irrigation pipes, and transportation.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A96063; ISO AlMg0.5Si; Aluminium 6063-T835; AA6063-T835; Al6063-T835
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.70 g/cc0.0975 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 105105500 kg load with 10 mm ball
Hardness, Knoop 130130Converted from Brinell Hardness Value
Hardness, Rockwell A 4343Converted from Brinell Hardness Value
Hardness, Rockwell B 6666Converted from Brinell Hardness Value
Hardness, Vickers 118118Converted from Brinell Hardness Value
Tensile Strength, Ultimate 330 MPa47900 psi
Tensile Strength, Yield 295 MPa42800 psi
Elongation at Break 8.0 %8.0 %
Modulus of Elasticity 69.0 GPa10000 ksiAverage of Tension and Compression. In Al alloys, the compressive modulus is typically 2% greater than the tensile modulus
Poissons Ratio 0.330.33
Shear Modulus 25.8 GPa3740 ksi
Shear Strength 205 MPa29700 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000330 ohm-cm0.00000330 ohm-cmEstimated from other heat treatments.
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.1 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.4 µm/m-°C
@Temperature 20.0 - 100 °C
13.0 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 24.5 µm/m-°C
@Temperature 20.0 - 200 °C
13.6 µin/in-°F
@Temperature 68.0 - 392 °F
 25.6 µm/m-°C
@Temperature 20.0 - 300 °C
14.2 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.900 J/g-°C0.215 BTU/lb-°F
Thermal Conductivity 200 W/m-K1390 BTU-in/hr-ft²-°FEstimated from other heat treatments.
Melting Point 616 - 654 °C1140 - 1210 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 616 °C1140 °FAA; Typical
Liquidus 654 °C1210 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °Fhold at temperature for 2 to 3 hr; cool at 50°F per hour from 775 to 500°F
Solution Temperature 521 °C970 °F
Aging Temperature 177 °C350 °Fhold at temperature for 8 hr
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 97.5 %<= 97.5 %As remainder
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu <= 0.10 %<= 0.10 %
Iron, Fe <= 0.35 %<= 0.35 %
Magnesium, Mg 0.45 - 0.90 %0.45 - 0.90 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 0.20 - 0.60 %0.20 - 0.60 %
Titanium, Ti <= 0.10 %<= 0.10 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6063-T6
Aluminum 6063-O
Aluminum 6063-T83
Aluminum 6063-T832
Aluminum 6063-T831

MA6063T835 / 9404

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.