MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lubrizol Stat-Rite® X-5065 Static Control IDP-TPU Elastomeric Polymer Alloy
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane TPE; Polyurethane, TP

Material Notes: Elastomeric Stat-Rite® Polymer alloy X-5065 blend is a patented inherently dissipative polymer (IDP) with thermoplastic polyurethanes (TPU). This produces soft, flexible polymer alloys with an inherent static dissipative polymer network. This inherent static dissipative network remains intact through injection molding or extruding while maintaining the physical properties of TPU. Stat-Rite® TPU alloys are formulated for permanent and consistent ESD protection without comprising cleanliness.

Features:

  • Permanently static dissipative
  • Does not require humidity
  • Ultra-Clean: low off-gassing, low ionics, low particulates
  • See-through clarity
  • No particulates

Applications:

  • Cleanroom soft walls, windows and doors
  • Electronic component handling
  • Vacuum Tubing
  • Work surface mats

Properties of all Stat-Rite® polymer products in the molten state are adversely affected by moisture. Although Stat-Rite® compounds are dry when packaged, trace amounts of moisture can be absorbed during storage and handling. For best results, always dry the material two to three hours at 105°C (220°F) in a dehumidifying hopper dryer.

Data provided by Noveon, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9595ASTM D2240
Tensile Strength, Yield 37.9 MPa5500 psiASTM D412
Elongation at Break 700 %700 %ASTM D412
100% Modulus 10.3 MPa
@Strain 100 %
1500 psi
@Strain 100 %
ASTM D412
300% Modulus 19.3 MPa
@Strain 300 %
2800 psi
@Strain 300 %
ASTM D412
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1.00e+10 ohm1.00e+10 ohmASTM D257
Static Decay 0.20 sec0.20 sec50% R.H. Charge Plate Monitor
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 80 %80 %Mfr. Specifies transparent but doesn't quantify
 
Processing PropertiesMetricEnglishComments
Drying Temperature 105 °C221 °F
Dry Time 2 - 3 hour2 - 3 hour
 
Descriptive Properties
ColorTransparent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Taiwan Sheen Soon Sheenthane® D6610 Thermoplastic Polyurethane Elastomer
Huntsman IROGRAN® D 60 E 4024 Polyester-Based TPU-High Performance Grade
RTP Company RTP 1200 S-65D S-95833 Ester-based Thermoplastic Polyurethane Elastomer
Taiwan Sheen Soon Sheenthane® D6010 Thermoplastic Polyurethane Elastomer
Alliance Polymers Zythane™ 4065D Thermoplastic Polyurethane Elastomer

PNOVEON26 / 55456

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.