MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior Durethan® B 30 S 000000 Nylon 6 (PA6), Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: PA 6, injection molding-grade, non-reinforced, easy-flow, easy-release, rapid solidification

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³ISO 1183
Moisture Absorption at Equilibrium 3.0 %3.0 %50% RH; ISO 62
Water Absorption at Saturation 10 %10 %ISO 62
Linear Mold Shrinkage, Flow 0.012 cm/cm0.012 in/in150x105x3; 260 °C / MT 80 °C; 500 bar; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0116 cm/cm0.0116 in/in150x105x3; 260 °C / MT 80 °C; 500 bar; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 50.0 MPa7250 psiISO 2093-1
Tensile Strength, Yield 40.0 MPa5800 psi50 mm/min; ISO 527-1,-2
Elongation at Break >= 50 %>= 50 %50 mm/min, Nominal; ISO 527-1,-2
Elongation at Yield 20 %20 %50 mm/min; ISO 527-1,-2
Tensile Modulus 1.00 GPa145 ksi1 mm/min; ISO 527-1,-2
Flexural Strength 35.0 MPa5080 psi2 mm/min; ISO 178-A
Flexural Yield Strength 25.0 MPa
@Strain 3.5 %
3630 psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 0.850 GPa123 ksi2 mm/min; ISO 178-A
Flexural Strain at Break 8.0 %8.0 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) <= 10.0 kJ/m²
@Temperature 23.0 °C
<= 4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Izod Impact, Unnotched (ISO)  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 180-1U
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 180-1U
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179-1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179-1eU
Charpy Impact, Notched  <= 1.00 J/cm²
@Temperature -30.0 °C
<= 4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 179 1eA
 2.00 J/cm²
@Temperature 23.0 °C
9.52 ft-lb/in²
@Temperature 73.4 °F
ISO 179 1eA
Tensile Creep Modulus, 1 hour 800 MPa116000 psiISO 899-1
Tensile Creep Modulus, 1000 hours 600 MPa87000 psiISO 899-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+10 ohm-cm1.00e+10 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 60093
Dielectric Constant  4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
IEC 60250
 15
@Frequency 100 Hz
15
@Frequency 100 Hz
IEC 60250
Dielectric Strength 30.0 kV/mm
@Thickness 1.00 mm
762 kV/in
@Thickness 0.0394 in
IEC 60243-1
Dissipation Factor  0.12
@Frequency 1e+6 Hz
0.12
@Frequency 1e+6 Hz
IEC 60250
 0.20
@Frequency 100 Hz
0.20
@Frequency 100 Hz
IEC 60250
 
Thermal PropertiesMetricEnglishComments
Melting Point 222 °C432 °F10°C/min (Dry); ISO 11357-1,-3
 
Processing PropertiesMetricEnglishComments
Melt Temperature 270 °C518 °Finjection molding; ISO 294
 260 - 280 °C500 - 536 °F
Mold Temperature 80.0 °C176 °Finjection molding; ISO 294
 80.0 - 100 °C176 - 212 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Envalior Durethan® B 30 S 000000 Nylon 6 (PA6), Dry
BASF Ultramid® 8267G HS BK-106 15/25% Glass/Mineral Filled PA6 (Dry)
Envalior Akulon® K222-D PA6, Conditioned, Low Viscosity
Envalior Akulon® K222-D PA6, Dry, Low Viscosity
Envalior Akulon® K224-G6U (Cond.) 33% Glass Reinforced Nylon 6 (North America)

PLANW9257 / 208058

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.