MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Overview of materials for Polyphenylene Sulfide (PPS) with 20% Glass Fiber Filler
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 20% Glass Fiber Filler

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyphenylene Sulfide (PPS) with 20% Glass Fiber Filler". Specific grades with glass content between 15% and 24% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.30 - 2.53 g/cc0.0470 - 0.0914 lb/in³Average value: 1.51 g/cc Grade Count:31
Filler Content 15.0 - 20.0 %15.0 - 20.0 %Average value: 18.0 % Grade Count:5
Water Absorption 0.0200 - 0.0700 %0.0200 - 0.0700 %Average value: 0.0255 % Grade Count:11
 0.0300 - 0.0300 %
@Temperature -17.8 - -17.8 °C
0.0300 - 0.0300 %
@Temperature 0.000 - 0.000 °F
Average value: 0.0300 % Grade Count:1
Water Absorption at Saturation 0.0200 %0.0200 %Average value: 0.0200 % Grade Count:8
Additive Loading 20.0 %20.0 %Average value: 20.0 % Grade Count:4
Maximum Moisture Content 0.0200 - 0.05000.0200 - 0.0500Average value: 0.0300 Grade Count:3
Linear Mold Shrinkage 0.000500 - 0.00800 cm/cm0.000500 - 0.00800 in/inAverage value: 0.00347 cm/cm Grade Count:22
Linear Mold Shrinkage, Transverse 0.00300 - 0.0100 cm/cm0.00300 - 0.0100 in/inAverage value: 0.00644 cm/cm Grade Count:9
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 100 - 102100 - 102Average value: 101 Grade Count:3
Hardness, Rockwell R 121 - 125121 - 125Average value: 122 Grade Count:3
Tensile Strength, Ultimate 86.0 - 162 MPa12500 - 23500 psiAverage value: 116 MPa Grade Count:29
Elongation at Break 0.860 - 3.00 %0.860 - 3.00 %Average value: 1.74 % Grade Count:30
Modulus of Elasticity 5.00 - 23.4 GPa725 - 3400 ksiAverage value: 10.1 GPa Grade Count:20
Flexural Yield Strength 113 - 231 MPa16400 - 33500 psiAverage value: 171 MPa Grade Count:28
Flexural Modulus 5.10 - 25.0 GPa740 - 3630 ksiAverage value: 8.96 GPa Grade Count:31
Flexural Strain at Break 0.800 - 4.50 %0.800 - 4.50 %Average value: 2.41 % Grade Count:5
Izod Impact, Notched 0.427 - 3.20 J/cm0.800 - 6.00 ft-lb/inAverage value: 0.873 J/cm Grade Count:15
Izod Impact, Unnotched 2.14 - 3.74 J/cm4.00 - 7.00 ft-lb/inAverage value: 2.84 J/cm Grade Count:9
Izod Impact, Notched (ISO) 5.20 - 35.0 kJ/m²2.47 - 16.7 ft-lb/in²Average value: 10.9 kJ/m² Grade Count:6
Charpy Impact Unnotched 1.10 - 6.00 J/cm²5.24 - 28.6 ft-lb/in²Average value: 4.03 J/cm² Grade Count:11
Charpy Impact, Notched 0.320 - 1.81 J/cm²1.52 - 8.60 ft-lb/in²Average value: 1.01 J/cm² Grade Count:13
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 10.0 - 2.20e+16 ohm-cm10.0 - 2.20e+16 ohm-cmAverage value: 6.49e+15 ohm-cm Grade Count:15
Surface Resistance 1000 - 9.80e+15 ohm1000 - 9.80e+15 ohmAverage value: 1.97e+15 ohm Grade Count:6
Dielectric Constant 3.20 - 5.003.20 - 5.00Average value: 3.80 Grade Count:10
Dielectric Strength 13.8 - 30.0 kV/mm350 - 762 kV/inAverage value: 18.9 kV/mm Grade Count:11
Dissipation Factor 0.00100 - 0.007000.00100 - 0.00700Average value: 0.00360 Grade Count:10
Arc Resistance 100 - 120 sec100 - 120 secAverage value: 113 sec Grade Count:3
Comparative Tracking Index 125 - 200 V125 - 200 VAverage value: 180 V Grade Count:5
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 - 29.0 µm/m-°C6.67 - 16.1 µin/in-°FAverage value: 23.3 µm/m-°C Grade Count:8
 12.0 - 60.0 µm/m-°C
@Temperature 100 - 200 °C
6.67 - 33.3 µin/in-°F
@Temperature 212 - 392 °F
Average value: 27.8 µm/m-°C Grade Count:4
CTE, linear, Transverse to Flow 49.0 - 75.0 µm/m-°C27.2 - 41.7 µin/in-°FAverage value: 60.1 µm/m-°C Grade Count:5
 130 - 150 µm/m-°C
@Temperature 100 - 200 °C
72.2 - 83.3 µin/in-°F
@Temperature 212 - 392 °F
Average value: 140 µm/m-°C Grade Count:2
Melting Point 278 - 280 °C532 - 536 °FAverage value: 279 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 246 - 280 °C475 - 536 °FAverage value: 261 °C Grade Count:5
Deflection Temperature at 1.8 MPa (264 psi) 165 - 275 °C329 - 527 °FAverage value: 249 °C Grade Count:29
Flammability, UL94 HB - V-0HB - V-0Grade Count:18
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 340 °C68.0 - 644 °FAverage value: 231 °C Grade Count:11
Nozzle Temperature 299 - 330 °C570 - 626 °FAverage value: 321 °C Grade Count:5
Die Temperature 310 - 330 °C590 - 626 °FAverage value: 320 °C Grade Count:4
Melt Temperature 288 - 349 °C550 - 660 °FAverage value: 319 °C Grade Count:21
Mold Temperature 65.6 - 177 °C150 - 350 °FAverage value: 146 °C Grade Count:21
Drying Temperature 80.0 - 150 °C176 - 302 °FAverage value: 135 °C Grade Count:20
Moisture Content 0.0200 - 0.0400 %0.0200 - 0.0400 %Average value: 0.0307 % Grade Count:15
Injection Pressure 30.0 - 103 MPa4350 - 15000 psiAverage value: 81.5 MPa Grade Count:14

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyphenylene Sulfide (PPS) with 30% Glass Fiber Filler
Overview of materials for Polyphenylene Sulfide (PPS) with 10% Glass Fiber Filler
Overview of materials for Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler
Overview of materials for Polyphenylene Sulfide (PPS) with 50% Glass Fiber Filler
Overview of materials for Polyphenylene Sulfide (PPS), Unreinforced, Extruded

O4512 / 78339

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.