MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Zotefoams Evazote® EV50 Ethylene Vinyl Acetate Copolymer Foam
Categories: Polymer; Thermoplastic; Ethylene Vinyl Acetate

Material Notes: Evazote® is a closed cell, cross-linked EVA copolymer foam manufactured using nitrogen expansion technology to produce foams with exceptional cell size uniformity, low odor / high purity and outstanding physical attributes.

Information provided by Zotefoams

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.0410 - 0.0540 g/cc0.00148 - 0.00195 lb/in³sheet density
 0.0500 g/cc0.00181 lb/in³Nominal skin/skin; BS ISO 7214 1998
Cell Length 0.350 mm0.0138 inTypical Diameter
 0.250 - 0.600 mm0.00984 - 0.0236 in
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore OO 474710 mm cell/cell thickness; ISO 868 1985
Tensile Strength 0.840 MPa122 psiISO 7214 1998
Elongation at Break 245 %245 %
Compressive Yield Strength  0.0300 MPa
@Strain 10 %
4.35 psi
@Strain 10 %
BS ISO 7214 1998
 0.0510 MPa
@Strain 25 %
7.40 psi
@Strain 25 %
BS ISO 7214 1998
 0.0820 MPa
@Strain 40 %
11.9 psi
@Strain 40 %
BS ISO 7214 1998
 0.115 MPa
@Strain 50 %
16.7 psi
@Strain 50 %
BS ISO 7214 1998
Tear Strength 1.055 kN/m6.020 pliBS EN ISO 8067 1995
Compression Set  3.0 %
@Time 79200 sec,
Strain 25 %
3.0 %
@Time 22.0 hour,
Strain 25 %
24 hr recovery; BS ISO 7214 1998
 10.5 %
@Time 79200 sec,
Strain 25 %
10.5 %
@Time 22.0 hour,
Strain 25 %
0.5 hr recovery; BS ISO 7214 1998
 13 %
@Time 79200 sec,
Strain 50 %
13 %
@Time 22.0 hour,
Strain 50 %
24 hr recovery; BS ISO 7214 1998
 23.5 %
@Time 79200 sec,
Strain 50 %
23.5 %
@Time 22.0 hour,
Strain 50 %
0.5 hr recovery; BS ISO 7214 1998
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.0404 W/m-K0.280 BTU-in/hr-ft²-°Fmean temp of 10°C; ISO 8302 1991
Maximum Service Temperature, Air 65.0 °C149 °F
Minimum Service Temperature, Air -70.0 °C-94.0 °F
Flammability Test  0.80
@Thickness 13.0 mm
0.80
@Thickness 0.512 in
Horizontal Burn Rate, mm/sec; ISO 7214 1998
 1.0
@Thickness 5.00 mm
1.0
@Thickness 0.197 in
Horizontal Burn Rate, mm/sec; ISO 7214 1998
Shrinkage  3.0 %
@Temperature 70.0 °C,
Time 3600 sec
3.0 %
@Temperature 158 °F,
Time 1.00 hour
 3.5 %
@Temperature 70.0 °C,
Time 360000 sec
3.5 %
@Temperature 158 °F,
Time 100 hour
 4.0 %
@Temperature 70.0 °C,
Time 3.60e+6 sec
4.0 %
@Temperature 158 °F,
Time 1000 hour
 6.5 %
@Temperature 80.0 °C,
Time 3600 sec
6.5 %
@Temperature 176 °F,
Time 1.00 hour
 10 %
@Temperature 80.0 °C,
Time 36000 sec
10 %
@Temperature 176 °F,
Time 10.0 hour
 12.5 %
@Temperature 80.0 °C,
Time 180000 sec
12.5 %
@Temperature 176 °F,
Time 50.0 hour
 
Descriptive Properties
FlammabilityAutomotive: FMVSS.302 burn ratePass: 4mm and thicker

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Zotefoams Supazote® EM26 Lightweight Supersoft Ethylene Copolymer Foam
Zotefoams Evazote® EV30 Ethylene Vinyl Acetate Copolymer Foam
Overview of materials for Ethylene Vinyl Acetate Copolymer (EVA), Film Grade
Overview of materials for Ethylene Vinyl Acetate Copolymer (EVA), Extrusion/Coating Grade
Zotefoams Plastazote® HD30 High Density Polyethylene Foam

PZOTEF945 / 150701

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.