MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Westlake EBAC® SP1806 17.5%, Ethylene-Methyl Acrylate Copolymer
Categories: Polymer; Thermoplastic; Ethylene Butyl Acrylate

Material Notes: Description: Westlake EBAC® SP1806 is an ethylene butyl acrylate copolymer designed for extrusion coating and laminating. SP1806 can also be compounded as an impact modifier or used in highly filled applications. Westlake EBAC® resins are less crystalline and softer than polyethylene and offer compatibility and adhesion to typically difficult to bond to polymers. SP1806 is non-corrosive at extrusion temperatures and has excellent thermal stability.
    Key Attributes:
  • Good adhesion/compatibility to various substrates
  • Good heat and RF sealing
  • Low temperature toughness
  • Soft, flexible, tough without plasticizer
    Application/Uses:
  • Extrusion coating / laminations
  • Flexible Packaging
  • Impact Modifier
  • Compounding / high filler loadings

Information provided by Westlake Chemical

Key Words: Good adhesion/compatibility to various substrates
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.925 g/cc0.0334 lb/in³ASTM D1505
Butyl Acrylate Content 17.5 %17.5 %Westlake
Melt Flow 7.3 g/10 min
@Load 2.16 kg,
Temperature 190 °C
7.3 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4040ASTM D2240
Tensile Strength at Break 10.0 MPa1450 psi50 mm/min; ASTM D 638 Type IV Specimen
Elongation at Break 730 %730 %50 mm/min; ASTM D 638 Type IV Specimen
 
Thermal PropertiesMetricEnglishComments
Melting Point 91.0 °C196 °Fby DSC; ASTM D3418
Vicat Softening Point 55.0 °C131 °FASTM D1525
Brittleness Temperature <= -73.0 °C<= -99.4 °FASTM D746
 
Descriptive Properties
ProcessCoating
 Extrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Westlake EBAC® Plus SP1903 18% Ethylene Butyl Acrylate Copolymer
Westlake EMAC® SA2413 Ethylene Methyl Acrylate Copolymer
Dow Elvaloy® 3117 AC Ethylene and 17% Butyl Acrylate Copolymer
Lucobit Lucofin® 1400MN Ethylene Butyl Acrylate
LyondellBasell Lucalen A2910M Low Density Polyethylene

PWESF8901 / 133446

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.