MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Makrolon® EM 9417 Polycarbonate, 10% Glass Fiber
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, 10% Glass Filled

Material Notes: MVR (300 °C/1.2 kg) 6.0 cm³/10 min; 10 % glass fiber reinforced; flame retardant; high viscosity; UV stabilized; easy release; injection molding - melt temperature 310 - 330 °C; available in opaque colors only

Mechanical property data for samples at 50% RH.

Information provided by Covestro.

Key Words: EM9417
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.27 g/cc0.0459 lb/in³ISO 1183-1
Linear Mold Shrinkage 0.0050 cm/cm
@Pressure 50.0 MPa
0.0050 in/in
@Pressure 7250 psi
60x60x2 mm; ISO 294-4
Linear Mold Shrinkage, Flow 0.0060 cm/cm
@Pressure 50.0 MPa
0.0060 in/in
@Pressure 7250 psi
60x60x2 mm; ISO 294-4
Melt Flow 7.62 g/10 min
@Load 1.20 kg,
Temperature 300 °C
7.62 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 45.0 MPa6530 psi50mm/min; ISO 527-1,-2
Tensile Strength, Yield 60.0 MPa8700 psi50mm/min; ISO 527-1,-2
Elongation at Break 15 %15 %5mm/min, complete break; ISO 524-1,-2
Elongation at Yield 5.0 %5.0 %50mm/min; ISO 527-1,-2
Tensile Modulus 3.70 GPa
@Temperature 23.0 °C
537 ksi
@Temperature 73.4 °F
1mm/min, complete break; ISO 527-1,-2
Charpy Impact Unnotched >= 7.50 J/cm²
@Temperature 23.0 °C
>= 35.7 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eU
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmIEC 60093
Surface Resistance 1.00e+16 ohm1.00e+16 ohmIEC 60093
Comparative Tracking Index 175 V175 Vsolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 40.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
22.2 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow 60.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
33.3 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Deflection Temperature at 0.46 MPa (66 psi) 141 °C286 °Fcomplete break; ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 135 °C275 °Fcomplete break; ISO 75-1,-2
Vicat Softening Point  143 °C
@Load 5.10 kg
289 °F
@Load 11.2 lb
@ 50°C/h; ISO 306
 144 °C
@Load 5.10 kg
291 °F
@Load 11.2 lb
@ 120°C/h; ISO 306
UL RTI, Electrical 125 °C
@Thickness 1.50 mm
257 °F
@Thickness 0.0591 in
UL RTI, Mechanical with Impact 115 °C
@Thickness 1.50 mm
239 °F
@Thickness 0.0591 in
UL RTI, Mechanical without Impact 125 °C
@Thickness 1.50 mm
257 °F
@Thickness 0.0591 in
Flammability, UL94 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
UL 94
Oxygen Index 35 %35 %Method A; ISO 4589-2
Glow Wire Flammability Index 960 °C
@Thickness 1.50 mm
1760 °F
@Thickness 0.0591 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Melt Temperature 300 °C572 °Finjection molding; ISO 294
Mold Temperature 110 °C230 °Finjection molding; ISO 294
Injection Velocity 200 mm/sec7.87 in/secinjection molding; ISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Makrolon® RW 2405 Polycarbonate, 10% Glass Fiber
MRC Polymers NAXELL™ PC110-10G General Purpose Polycarbonate, 10% Glass Fiber Filled, Medium Viscosity
Overview of materials for Polycarbonate, 10% Glass Filled
Covestro Makrolon® RW 2407 Polycarbonate
A. Schulman ComAlloy® 510-3010 10% Glass Fiber Reinforced Polycarbonate

PB095065 / 200135

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.