MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LG Chemical LUMID HI1102A(W) PA6, High Impact
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Impact Grade

Material Notes: Feature: Injection Molding, PA6, High Impact

Application: H/Lamp Screw Mounting

CAS No. 25038-54-4 and 9010-79-1

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.10 g/cc1.10 g/ccASTM D792
Water Absorption 1.4 %1.4 %ASTM D570
Linear Mold Shrinkage, Flow 0.012 - 0.016 cm/cm
@Thickness 3.20 mm
0.012 - 0.016 in/in
@Thickness 0.126 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 114114ASTM D785
Tensile Strength, Yield 66.7 MPa
@Thickness 3.20 mm
9670 psi
@Thickness 0.126 in
50mm/min; ASTM D638
Elongation at Break 80 %
@Thickness 3.20 mm
80 %
@Thickness 0.126 in
50mm/min; ASTM D638
Flexural Yield Strength 83.4 MPa
@Thickness 3.20 mm
12100 psi
@Thickness 0.126 in
2.8mm/min; ASTM D790
Flexural Modulus 2.16 GPa
@Thickness 3.20 mm
313 ksi
@Thickness 0.126 in
2.8mm/min; ASTM D790
Izod Impact, Notched 1.67 J/cm
@Thickness 6.40 mm,
Temperature 23.0 °C
3.12 ft-lb/in
@Thickness 0.252 in,
Temperature 73.4 °F
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmASTM D257
Dielectric Constant 2.8
@Frequency 1e+6 Hz
2.8
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 19.0 kV/mm
@Thickness 1.00 mm
483 kV/in
@Thickness 0.0394 in
ASTM D149
Arc Resistance 195 sec195 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 100 µm/m-°C55.6 µin/in-°FASTM D696
Melting Point 220 °C428 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 150 °C
@Thickness 6.40 mm
302 °F
@Thickness 0.252 in
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 50.0 °C
@Thickness 6.40 mm
122 °F
@Thickness 0.252 in
Unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 230 - 260 °C446 - 500 °FInjection Molding
Middle Barrel Temperature 240 - 270 °C464 - 518 °FInjection Molding
Front Barrel Temperature 250 - 280 °C482 - 536 °FInjection Molding
Nozzle Temperature 250 - 280 °C482 - 536 °FInjection Molding
Melt Temperature 250 - 280 °C482 - 536 °FInjection Molding
Mold Temperature 60.0 - 80.0 °C140 - 176 °FInjection Molding
Drying Temperature 80.0 - 100 °C176 - 212 °FInjection Molding
Dry Time 4.00 - 5.00 hour4.00 - 5.00 hourInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical LUMID HI1102B(W) PA66, High Impact
LG Chemical LUMID HI1202A(W) PA6, High Impact
LG Chemical LUMID HI1202B(W) PA66, High Impact
LG Chemical LUMID GP1100A(W) PA6, Low Viscosity
LG Chemical LUMID HI5006A(W) PA6/ABS, High Impact, Good Dimensional Stability

PLAY123 / 148131

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.