Physical Properties | Metric | English | Comments |
---|
Density | 1.48 g/cc | 0.0535 lb/in³ |
Moisture Absorption | 2.20 % | 2.20 % |
Linear Mold Shrinkage, Flow | 0.0050 cm/cm | 0.0050 in/in |
Linear Mold Shrinkage, Transverse | 0.010 cm/cm | 0.010 in/in |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 210 MPa | 30500 psi |
| 60.0 MPa @Temperature 200 °C | 8700 psi @Temperature 392 °F |
| 75.0 MPa @Temperature 180 °C | 10900 psi @Temperature 356 °F |
| 85.0 MPa @Temperature 160 °C | 12300 psi @Temperature 320 °F |
| 100 MPa @Temperature 120 °C | 14500 psi @Temperature 248 °F |
Elongation at Break | 3.0 % | 3.0 % |
| 10 % @Temperature 120 °C | 10 % @Temperature 248 °F |
| 11 % @Temperature 160 °C | 11 % @Temperature 320 °F |
| 12 % @Temperature 180 °C | 12 % @Temperature 356 °F |
| 12.5 % @Temperature 200 °C | 12.5 % @Temperature 392 °F |
Tensile Modulus | 13.0 GPa | 1890 ksi |
| 3.40 GPa @Temperature 200 °C | 493 ksi @Temperature 392 °F |
| 4.20 GPa @Temperature 180 °C | 609 ksi @Temperature 356 °F |
| 4.60 GPa @Temperature 160 °C | 667 ksi @Temperature 320 °F |
| 5.00 GPa @Temperature 120 °C | 725 ksi @Temperature 248 °F |
Flexural Modulus | 13.0 GPa | 1890 ksi |
| 3.40 GPa @Temperature 200 °C | 493 ksi @Temperature 392 °F |
| 4.20 GPa @Temperature 180 °C | 609 ksi @Temperature 356 °F |
| 4.60 GPa @Temperature 160 °C | 667 ksi @Temperature 320 °F |
| 5.00 GPa @Temperature 120 °C | 725 ksi @Temperature 248 °F |
Izod Impact, Notched (ISO) | 15.0 kJ/m² @Temperature 23.0 °C | 7.14 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact Unnotched | 6.50 J/cm² @Temperature -30.0 °C | 30.9 ft-lb/in² @Temperature -22.0 °F |
| 9.00 J/cm² @Temperature 23.0 °C | 42.8 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact, Notched | 1.20 J/cm² @Temperature -30.0 °C | 5.71 ft-lb/in² @Temperature -22.0 °F |
| 1.50 J/cm² @Temperature 23.0 °C | 7.14 ft-lb/in² @Temperature 73.4 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Comparative Tracking Index | 300 V | 300 V |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 25.0 µm/m-°C | 13.9 µin/in-°F |
CTE, linear, Transverse to Flow | 50.0 µm/m-°C | 27.8 µin/in-°F |
Melting Point | 282 °C | 540 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 256 °C | 493 °F |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.