Physical Properties | Metric | English | Comments |
---|
Density | 7.75 g/cc | 0.280 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell B | 82.3 @Temperature 23.0 °C | 82.3 @Temperature 73.4 °F |
Tensile Strength, Ultimate | 762 MPa @Temperature 23.0 °C | 111000 psi @Temperature 73.4 °F |
Tensile Strength, Yield | 364 MPa @Strain 0.2 %, Temperature 20.0 °C | 52800 psi @Strain 0.2 %, Temperature 68.0 °F |
| 364 MPa @Strain 0.2 %, Thickness 0.500 mm | 52800 psi @Strain 0.2 %, Thickness 0.0197 in |
Elongation at Break | 37.5 % @Thickness 0.500 mm, Temperature 20.0 °C | 37.5 % @Thickness 0.0197 in, Temperature 68.0 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000080280 ohm-cm @Temperature 22.0 °C | 0.000080280 ohm-cm @Temperature 71.6 °F |
| 0.000084609 ohm-cm @Temperature 93.0 °C | 0.000084609 ohm-cm @Temperature 199 °F |
| 0.000090800 ohm-cm @Temperature 204 °C | 0.000090800 ohm-cm @Temperature 399 °F |
| 0.000096000 ohm-cm @Temperature 315 °C | 0.000096000 ohm-cm @Temperature 599 °F |
| 0.0001010 ohm-cm @Temperature 427 °C | 0.0001010 ohm-cm @Temperature 801 °F |
| 0.00010601 ohm-cm @Temperature 538 °C | 0.00010601 ohm-cm @Temperature 1000 °F |
| 0.00011060 ohm-cm @Temperature 649 °C | 0.00011060 ohm-cm @Temperature 1200 °F |
| 0.00011493 ohm-cm @Temperature 760 °C | 0.00011493 ohm-cm @Temperature 1400 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 16.61 µm/m-°C @Temperature 100 °C | 9.228 µin/in-°F @Temperature 212 °F |
| 16.78 µm/m-°C @Temperature 200 °C | 9.322 µin/in-°F @Temperature 392 °F |
| 17.02 µm/m-°C @Temperature 300 °C | 9.456 µin/in-°F @Temperature 572 °F |
| 17.26 µm/m-°C @Temperature 400 °C | 9.589 µin/in-°F @Temperature 752 °F |
| 17.45 µm/m-°C @Temperature 500 °C | 9.694 µin/in-°F @Temperature 932 °F |
| 17.48 µm/m-°C @Temperature 700 °C | 9.711 µin/in-°F @Temperature 1290 °F |
| 17.69 µm/m-°C @Temperature 600 °C | 9.828 µin/in-°F @Temperature 1110 °F |
Specific Heat Capacity | 0.472 J/g-°C @Temperature 23.0 °C | 0.113 BTU/lb-°F @Temperature 73.4 °F |
| 0.497 J/g-°C @Temperature 100 °C | 0.119 BTU/lb-°F @Temperature 212 °F |
| 0.540 J/g-°C @Temperature 300 °C | 0.129 BTU/lb-°F @Temperature 572 °F |
| 0.572 J/g-°C @Temperature 500 °C | 0.137 BTU/lb-°F @Temperature 932 °F |
| 0.597 J/g-°C @Temperature 700 °C | 0.143 BTU/lb-°F @Temperature 1290 °F |
| 0.618 J/g-°C @Temperature 900 °C | 0.148 BTU/lb-°F @Temperature 1650 °F |
| 0.626 J/g-°C @Temperature 1000 °C | 0.150 BTU/lb-°F @Temperature 1830 °F |
| 0.638 J/g-°C @Temperature 1150 °C | 0.152 BTU/lb-°F @Temperature 2100 °F |
Thermal Conductivity | 14.189 W/m-K @Temperature 23.0 °C | 98.472 BTU-in/hr-ft²-°F @Temperature 73.4 °F |
| 15.561 W/m-K @Temperature 100 °C | 107.99 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 18.552 W/m-K @Temperature 300 °C | 128.75 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 21.393 W/m-K @Temperature 500 °C | 148.47 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 24.193 W/m-K @Temperature 700 °C | 167.90 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 26.926 W/m-K @Temperature 900 °C | 186.87 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 28.252 W/m-K @Temperature 1000 °C | 196.07 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 30.238 W/m-K @Temperature 1150 °C | 209.85 BTU-in/hr-ft²-°F @Temperature 2100 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 0.15 % | 0.15 % |
Carbon, C | <= 0.050 % | <= 0.050 % |
Chromium, Cr | 19.5 - 21 % | 19.5 - 21 % |
Copper, Cu | <= 0.75 % | <= 0.75 % |
Iron, Fe | 60.645 - 70.7 % | 60.645 - 70.7 % |
Manganese, Mn | 0.40 % | 0.40 % |
Molybdenum, Mo | 0.40 % | 0.40 % |
Nickel, Ni | 8.75 - 15.5 % | 8.75 - 15.5 % |
Silicon, Si | 0.70 % | 0.70 % |
Sulfur, S | <= 0.0050 % | <= 0.0050 % |
Titanium, Ti | 0.40 % | 0.40 % |
|
Descriptive Properties |
---|
Thermal Diffusivity (cm2/s) | 0.0385 |
| 0.0401 |
| 0.044 |
| 0.0479 |
| 0.0519 |
| 0.0558 |
| 0.0578 |
| 0.0607 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.