Physical Properties | Metric | English | Comments |
---|
Density | 1.35 - 1.80 g/cc | 0.0488 - 0.0650 lb/in³ |
| 1.24 - 1.24 g/cc @Temperature 270 - 270 °C | 0.0448 - 0.0448 lb/in³ @Temperature 518 - 518 °F |
Filler Content | 45.0 - 50.0 % | 45.0 - 50.0 % |
Water Absorption | 0.200 - 5.30 % | 0.200 - 5.30 % |
| 1.20 - 1.20 % @Temperature 70.0 - 70.0 °C | 1.20 - 1.20 % @Temperature 158 - 158 °F |
Moisture Absorption at Equilibrium | 0.200 - 4.80 % | 0.200 - 4.80 % |
| 1.20 - 1.60 % @Temperature 70.0 - 70.0 °C | 1.20 - 1.60 % @Temperature 158 - 158 °F |
| 0.450 - 1.00 % @Temperature 70.0 - 70.0 °C | 0.450 - 1.00 % @Temperature 158 - 158 °F |
| 0.450 - 1.00 % @Time 180000 - 1.44e+6 sec | 0.450 - 1.00 % @Time 50.0 - 400 hour |
Water Absorption at Saturation | 0.800 - 8.00 % | 0.800 - 8.00 % |
Viscosity | 2.90 - 3.00 cP | 2.90 - 3.00 cP |
| 100 - 400 cP @Temperature 230 - 270 °C | 100 - 400 cP @Temperature 446 - 518 °F |
| 100 - 400 cP @Shear Rate 100 - 1000 1/s | 100 - 400 cP @Shear Rate 100 - 1000 1/s |
Viscosity Test | 145 - 150 cm³/g | 1.45 - 1.50 dl/g |
Maximum Moisture Content | 0.150 - 0.200 | 0.150 - 0.200 |
| 0.200 - 0.200 @Temperature 120 - 120 °C | 0.200 - 0.200 @Temperature 248 - 248 °F |
| 0.200 - 0.200 @Time 299 - 299 sec | 0.200 - 0.200 @Time 0.0830 - 0.0830 hour |
Linear Mold Shrinkage | 0.000200 - 0.0150 cm/cm | 0.000200 - 0.0150 in/in |
| 0.00100 - 0.00300 cm/cm @Temperature 80.0 - 80.0 °C | 0.00100 - 0.00300 in/in @Temperature 176 - 176 °F |
Linear Mold Shrinkage, Transverse | 0.000700 - 0.0141 cm/cm | 0.000700 - 0.0141 in/in |
| 0.00500 - 0.00500 cm/cm @Temperature 80.0 - 80.0 °C | 0.00500 - 0.00500 in/in @Temperature 176 - 176 °F |
Melt Flow | 1.00 - 38.8 g/10 min | 1.00 - 38.8 g/10 min |
Spiral Flow | 34.0 - 50.0 cm | 13.4 - 19.7 in |
Ash | 38.0 - 52.0 % | 38.0 - 52.0 % |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell M | 95.0 - 109 | 95.0 - 109 |
Hardness, Rockwell R | 65.0 - 125 | 65.0 - 125 |
| 30.0 - 30.0 @Temperature 80.0 - 80.0 °C | 30.0 - 30.0 @Temperature 176 - 176 °F |
Hardness, Shore D | 78.0 - 84.0 | 78.0 - 84.0 |
Ball Indentation Hardness | 109 - 340 MPa | 15800 - 49300 psi |
Tensile Strength, Ultimate | 90.0 - 605 MPa | 13100 - 87700 psi |
| 55.0 - 321.64 MPa @Temperature -40.0 - 150 °C | 7980 - 46650 psi @Temperature -40.0 - 302 °F |
| 160 - 180 MPa @Temperature 70.0 - 70.0 °C | 23200 - 26100 psi @Temperature 158 - 158 °F |
| 160 - 180 MPa @Time 180000 - 1.44e+6 sec | 23200 - 26100 psi @Time 50.0 - 400 hour |
| 45.0 - 180 MPa @Strain 0.800 - 4.00 % | 6530 - 26100 psi @Strain 0.800 - 4.00 % |
| 45.0 - 180 MPa @Temperature 40.0 - 160 °C | 6530 - 26100 psi @Temperature 104 - 320 °F |
Tensile Strength, Yield | 126 - 240 MPa | 18300 - 34800 psi |
Elongation at Break | 1.00 - 8.00 % | 1.00 - 8.00 % |
| 2.30 - 9.00 % @Temperature -40.0 - 150 °C | 2.30 - 9.00 % @Temperature -40.0 - 302 °F |
Elongation at Yield | 1.00 - 5.00 % | 1.00 - 5.00 % |
Modulus of Elasticity | 7.49 - 30.1 GPa | 1090 - 4370 ksi |
| 3.80 - 15.9958 GPa @Temperature -40.0 - 150 °C | 551 - 2320.04 ksi @Temperature -40.0 - 302 °F |
Flexural Yield Strength | 175 - 840 MPa | 25400 - 122000 psi |
| 100 - 433.06 MPa @Temperature -40.0 - 121 °C | 14500 - 62810 psi @Temperature -40.0 - 250 °F |
Flexural Modulus | 1.60 - 26.5 GPa | 232 - 3840 ksi |
| 4.50 - 16.1 GPa @Temperature -40.0 - 121 °C | 653 - 2340 ksi @Temperature -40.0 - 250 °F |
Flexural Strain at Break | 3.00 - 5.00 % | 3.00 - 5.00 % |
Compressive Yield Strength | 120 - 274 MPa | 17400 - 39700 psi |
| 70.0 - 280 MPa @Temperature -40.0 - 80.0 °C | 10200 - 40600 psi @Temperature -40.0 - 176 °F |
Poissons Ratio | 0.170 - 0.340 | 0.170 - 0.340 |
Secant Modulus | 1.50 - 19.0 GPa @Temperature 40.0 - 160 °C | 218 - 2760 ksi @Temperature 104 - 320 °F |
| 1.50 - 19.0 GPa @Strain 0.000 - 4.00 % | 218 - 2760 ksi @Strain 0.000 - 4.00 % |
Izod Impact, Notched | 0.908 - 4.97 J/cm | 1.70 - 9.30 ft-lb/in |
| 1.15 - 5.97968 J/cm @Temperature -40.0 - 121 °C | 2.15 - 11.2024 ft-lb/in @Temperature -40.0 - 250 °F |
Izod Impact, Unnotched | 1.39 - 5340 J/cm | 2.60 - 10000 ft-lb/in |
Izod Impact, Notched (ISO) | 7.00 - 35.7 kJ/m² | 3.33 - 17.0 ft-lb/in² |
| 10.0 - 23.0 kJ/m² @Temperature -40.0 - -30.0 °C | 4.76 - 10.9 ft-lb/in² @Temperature -40.0 - -22.0 °F |
Izod Impact, Unnotched (ISO) | 70.0 kJ/m² - NB | 33.3 ft-lb/in² - NB |
| 75.0 kJ/m² - NB @Temperature -30.0 - -30.0 °C | 35.7 ft-lb/in² - NB @Temperature -22.0 - -22.0 °F |
Charpy Impact Unnotched | 1.00 J/cm² - NB | 4.76 ft-lb/in² - NB |
| 1.40 J/cm² - NB @Temperature -40.0 - -20.0 °C | 6.66 ft-lb/in² - NB @Temperature -40.0 - -4.00 °F |
Charpy Impact, Notched | 0.600 - 5.00 J/cm² | 2.86 - 23.8 ft-lb/in² |
| 0.800 - 2.50 J/cm² @Temperature -40.0 - -20.0 °C | 3.81 - 11.9 ft-lb/in² @Temperature -40.0 - -4.00 °F |
Puncture Energy | 3.60 - 14.0 J | 2.66 - 10.3 ft-lb |
| 3.40 - 6.00 J @Temperature -30.0 - -30.0 °C | 2.51 - 4.43 ft-lb @Temperature -22.0 - -22.0 °F |
Tensile Creep Modulus, 1 hour | 8100 - 14000 MPa | 1.17e+6 - 2.03e+6 psi |
Tensile Creep Modulus, 1000 hours | 6600 - 12000 MPa | 957000 - 1.74e+6 psi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 1.00e+9 - 1.00e+17 ohm-cm | 1.00e+9 - 1.00e+17 ohm-cm |
Surface Resistance | 1.00e+9 - 1.00e+16 ohm | 1.00e+9 - 1.00e+16 ohm |
Dielectric Constant | 3.00 - 14.2 | 3.00 - 14.2 |
Dielectric Strength | 7.87 - 80.0 kV/mm | 200 - 2030 kV/in |
Dissipation Factor | 0.00500 - 0.319 | 0.00500 - 0.319 |
Arc Resistance | 92.0 - 138 sec | 92.0 - 138 sec |
Comparative Tracking Index | 350 - 600 V | 350 - 600 V |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 2.00 - 149 µm/m-°C | 1.11 - 83.0 µin/in-°F |
| 13.0 - 15.0 µm/m-°C @Temperature 55.0 - 160 °C | 7.22 - 8.33 µin/in-°F @Temperature 131 - 320 °F |
| 12.0 - 16.0 µm/m-°C @Temperature 35.0 - 55.0 °C | 6.67 - 8.89 µin/in-°F @Temperature 95.0 - 131 °F |
| 12.0 - 16.0 µm/m-°C @Thickness 2.00 - 2.00 mm | 6.67 - 8.89 µin/in-°F @Thickness 0.0787 - 0.0787 in |
CTE, linear, Transverse to Flow | 18.0 - 121 µm/m-°C | 10.0 - 67.0 µin/in-°F |
| 69.0 - 69.0 µm/m-°C @Temperature 55.0 - 160 °C | 38.3 - 38.3 µin/in-°F @Temperature 131 - 320 °F |
Specific Heat Capacity | 1.00 - 1.40 J/g-°C | 0.239 - 0.335 BTU/lb-°F |
| 1.61 - 2.05 J/g-°C @Temperature 270 - 325 °C | 0.385 - 0.490 BTU/lb-°F @Temperature 518 - 617 °F |
Thermal Conductivity | 0.320 - 0.400 W/m-K | 2.22 - 2.78 BTU-in/hr-ft²-°F |
| 0.260 - 0.280 W/m-K @Temperature 270 - 325 °C | 1.80 - 1.94 BTU-in/hr-ft²-°F @Temperature 518 - 617 °F |
Melting Point | 178 - 325 °C | 352 - 617 °F |
Maximum Service Temperature, Air | 65.0 - 270 °C | 149 - 518 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 200 - 305 °C | 392 - 581 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 155 - 293 °C | 311 - 559 °F |
Deflection Temperature at 8.0 MPa | 140 - 210 °C | 284 - 410 °F |
Vicat Softening Point | 200 - 313 °C | 392 - 595 °F |
Minimum Service Temperature, Air | -60.0 - -30.0 °C | -76.0 - -22.0 °F |
Glass Transition Temp, Tg | 15.0 - 135 °C | 59.0 - 275 °F |
Decomposition Temperature | 300 - 350 °C | 572 - 662 °F |
UL RTI, Electrical | 65.0 °C | 149 °F |
UL RTI, Mechanical with Impact | 65.0 °C | 149 °F |
UL RTI, Mechanical without Impact | 65.0 °C | 149 °F |
Flammability, UL94 | HB | HB |
Flame Spread | 0.000 - 102 mm/min | 0.000 - 4.02 in/min |
Oxygen Index | 23.0 - 25.0 % | 23.0 - 25.0 % |
Glow Wire Test | 550 - 800 °C | 1020 - 1470 °F |
Ignition Temperature | 400 - 470 °C | 752 - 878 °F |
|
Processing Properties | Metric | English | Comments |
---|
Processing Temperature | 70.0 - 300 °C | 158 - 572 °F |
Nozzle Temperature | 230 - 293 °C | 446 - 560 °F |
Melt Temperature | 204 - 330 °C | 400 - 626 °F |
Mold Temperature | 26.7 - 180 °C | 80.0 - 356 °F |
Injection Velocity | 30.0 - 76.2 mm/sec | 1.18 - 3.00 in/sec |
Drying Temperature | 65.6 - 120 °C | 150 - 248 °F |
Moisture Content | 0.0300 - 0.200 % | 0.0300 - 0.200 % |
Dew Point | -28.9 - -17.8 °C | -20.0 - 0.000 °F |
Injection Pressure | 3.45 - 150 MPa | 500 - 21800 psi |