MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lubrizol Estane® 58610 Thermoplastic Polyurethane
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyester Grade

Material Notes: Features: Combines flexibility, toughness and excellent roll release for calendering and melt coating applications.

Uses: Injection molding and general extrusion techniques. It is used in film, sheet, coated fabric and laminations.

Available in Americas, Europe, Middle East, Africa, India and Asia

Information Provided by The Lubrizol Corporation

Key Words: TPU
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.22 g/cc1.22 g/ccASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8787ASTM D2240
 74
@Temperature 70.0 °C
74
@Temperature 158 °F
6 weeks, Heat Resistance
 75
@Temperature 100 °C
75
@Temperature 212 °F
10 weeks, Heat Resistance
 75
@Temperature 23.0 °C
75
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Shelf
 85
@Temperature 23.0 °C
85
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Arizona
 85
@Temperature 23.0 °C
85
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Florida
 85
@Temperature 23.0 °C
85
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Ohio
 85
@Temperature 23.0 °C
85
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Shelf
 85
@Temperature 23.0 °C
85
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Florida
 89
@Temperature 23.0 °C
89
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Ohio
 89
@Temperature 23.0 °C
89
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Arizona
Tensile Strength  4.05 MPa
@Temperature 70.0 °C
587 psi
@Temperature 158 °F
6 weeks, Heat Resistance
 5.79 MPa
@Temperature 23.0 °C
840 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Florida
 6.95 MPa
@Temperature 23.0 °C
1010 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Arizona
 8.11 MPa
@Temperature 23.0 °C
1180 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Ohio
 11.58 MPa
@Temperature 23.0 °C
1680 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Florida
 26.63 MPa
@Temperature 100 °C
3862 psi
@Temperature 212 °F
10 weeks, Heat Resistance
 32.42 MPa
@Temperature 23.0 °C
4702 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Arizona
 41.69 MPa
@Temperature 23.0 °C
6047 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Ohio
 59.06 MPa
@Temperature 23.0 °C
8566 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Shelf
 59.06 MPa
@Temperature 23.0 °C
8566 psi
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Shelf
Tensile Strength, Ultimate 57.9 MPa8400 psiASTM D412; ASTM D638
Elongation at Break 600 %600 %ASTM D412; ASTM D638
 222 %
@Temperature 23.0 °C
222 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Florida
 300 %
@Temperature 23.0 °C
300 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Arizona
 420 %
@Temperature 23.0 °C
420 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Ohio
 624 %
@Temperature 23.0 °C
624 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Florida
 630 %
@Temperature 23.0 °C
630 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Shelf
 654 %
@Temperature 23.0 °C
654 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 25 mil - Natural, Shelf
 690 %
@Temperature 100 °C
690 %
@Temperature 212 °F
10 weeks, Heat Resistance
 714 %
@Temperature 23.0 °C
714 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Ohio
 720 %
@Temperature 23.0 °C
720 %
@Temperature 73.4 °F
12 months, Weathering @ 45° South, 12 mil - Black, Arizona
 1080 %
@Temperature 70.0 °C
1080 %
@Temperature 158 °F
6 weeks, Heat Resistance
100% Modulus 6.10 MPa
@Strain 100 %
885 psi
@Strain 100 %
ASTM D412; ASTM D638
 4.10 MPa
@Strain 100 %,
Thickness 0.635 mm
595 psi
@Strain 100 %,
Thickness 0.0250 in
12 months, Weathering @ 45° South, Natural, Arizona
 4.40 MPa
@Strain 100 %,
Thickness 0.635 mm
638 psi
@Strain 100 %,
Thickness 0.0250 in
12 months, Weathering @ 45° South, Natural, Florida
 5.70 MPa
@Strain 100 %,
Thickness 0.305 mm
827 psi
@Strain 100 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Florida
 5.80 MPa
@Strain 100 %,
Thickness 0.635 mm
841 psi
@Strain 100 %,
Thickness 0.0250 in
12 months, Weathering @ 45° South, Natural, Ohio
 5.80 MPa
@Strain 100 %,
Thickness 0.305 mm
841 psi
@Strain 100 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Arizona
 6.20 MPa
@Strain 100 %,
Thickness 0.635 mm
899 psi
@Strain 100 %,
Thickness 0.0250 in
12 months, Weathering @ 45° South, Natural, Shelf
 6.20 MPa
@Strain 100 %,
Thickness 0.305 mm
899 psi
@Strain 100 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Ohio
 6.70 MPa
@Strain 100 %,
Thickness 0.305 mm
972 psi
@Strain 100 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Shelf
 3.70 MPa
@Treatment Temp. 70.0 °C,
Strain 100 %
537 psi
@Treatment Temp. 158 °F,
Strain 100 %
6 weeks, Heat Resistance
 4.00 MPa
@Treatment Temp. 100 °C,
Strain 100 %
580 psi
@Treatment Temp. 212 °F,
Strain 100 %
10 weeks, Heat Resistance
300% Modulus 9.00 MPa
@Strain 300 %
1310 psi
@Strain 300 %
ASTM D412; ASTM D638
 2.50 MPa
@Strain 300 %,
Thickness 0.635 mm
363 psi
@Strain 300 %,
Thickness 0.0250 in
12 months, Weathering @ 45° South, Natural, Ohio
 2.60 MPa
@Strain 300 %,
Thickness 0.305 mm
377 psi
@Strain 300 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Florida
 3.20 MPa
@Strain 300 %,
Thickness 0.305 mm
464 psi
@Strain 300 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Arizona
 3.50 MPa
@Strain 300 %,
Thickness 0.305 mm
508 psi
@Strain 300 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Ohio
 3.70 MPa
@Strain 300 %,
Thickness 0.635 mm
537 psi
@Strain 300 %,
Thickness 0.0250 in
12 months, Weathering @ 45° South, Natural, Shelf
 3.80 MPa
@Strain 300 %,
Thickness 0.305 mm
551 psi
@Strain 300 %,
Thickness 0.0120 in
12 months, Weathering @ 45° South, Black, Shelf
 2.60 MPa
@Treatment Temp. 100 °C,
Strain 300 %
377 psi
@Treatment Temp. 212 °F,
Strain 300 %
10 weeks, Heat Resistance
Flexural Stiffness 6.40 MPa
@Temperature 23.0 °C
928 psi
@Temperature 73.4 °F
ASTM D474
Taber Abrasion, mg/1000 Cycles 15
@Load 1.00 kg
15
@Load 2.20 lb
H-18 wheel; ASTM D1044
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 61.0 °C142 °FASTM D1525

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
NEU NEUSoft™ 596-50A Medical Ether TPU / SBC blend
NEU NEUSoft™ 597-50A Industrial Ether TPU / SBC blend
NEU NEUSoft™ 602-50A Ester TPU / SBC blend
Austin Novel Materials Texalan® 298A Polyester-based TPU
Lubrizol Estane® 58123 Thermoplastic Polyurethane

PNOVEON562 / 121453

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.