MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil LL 6201 Injection Molding Resin  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Injection Molded

Material Notes: LL 6201 is a narrow molecular weight butene copolymer designed for applications that require easy processability. This resin offers outstanding toughness and tear resistance in freezer applications for food packaging.

Information provided by ExxonMobil Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.926 g/cc0.0335 lb/in³ASTM D4883
ESCR 10% Igepal® <= 1.0 hour<= 1.0 hourCondition B; ASTM D1693
Melt Flow 50 g/10 min
@Load 2.16 kg,
Temperature 190 °C
50 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 11.2 MPa1630 psiASTM D638
Elongation at Break 90 %90 %ASTM D638
Flexural Modulus, 1% Secant 267 MPa38700 psiASTM D790
Tensile Impact Strength 220 kJ/m²
@Temperature -40.0 °C
105 ft-lb/in²
@Temperature -40.0 °F
ASTM D1822
 
Thermal PropertiesMetricEnglishComments
Melting Point 123 °C253 °FASTM D3418
Crystallization Temperature 108 °C226 °FASTM D3418
Vicat Softening Point 91.7 °C197 °FASTM D1525
Brittleness Temperature >= -70.0 °C>= -94.0 °FASTM D746

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil Escorene® LL-6101 LLDPE, Injection Grade
ExxonMobil LLDPE LL 6201XR Molding Linear Low Density Polyethylene Resin (European Grade)
ExxonMobil LLDPE LL 6201RQ Molding Linear Low Density Polyethylene Resin (European Grade)
ExxonMobil LL 6202 Injection Molding Resin
NOVA Chemicals Novapol® PF-0218-D Butene LLDPE Film Resin

PEXB208 / 37513

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.