Physical Properties | Metric | English | Comments |
---|
Density | 1.24 g/cc | 0.0448 lb/in³ |
Moisture Absorption | 0.80 - 0.90 % @Temperature 70.0 °C | 0.80 - 0.90 % @Temperature 158 °F |
Water Absorption at Saturation | 2.2 % | 2.2 % |
Linear Mold Shrinkage, Flow | 0.018 cm/cm | 0.018 in/in |
Linear Mold Shrinkage, Transverse | 0.021 cm/cm | 0.021 in/in |
Spiral Flow | 58.0 cm | 22.8 in |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Yield | 60.0 MPa | 8700 psi |
| 12.0 MPa @Temperature 80.0 °C | 1740 psi @Temperature 176 °F |
| 16.2 MPa @Temperature 80.0 °C | 2350 psi @Temperature 176 °F |
| 16.8 MPa @Temperature 80.0 °C | 2440 psi @Temperature 176 °F |
| 18.0 MPa @Temperature 80.0 °C | 2610 psi @Temperature 176 °F |
| 18.0 MPa @Temperature 80.0 °C | 2610 psi @Temperature 176 °F |
| 40.8 MPa @Temperature 23.0 °C | 5920 psi @Temperature 73.4 °F |
| 52.8 MPa @Temperature 23.0 °C | 7660 psi @Temperature 73.4 °F |
| 53.4 MPa @Temperature 23.0 °C | 7750 psi @Temperature 73.4 °F |
| 53.4 MPa @Temperature 23.0 °C | 7750 psi @Temperature 73.4 °F |
| 54.0 MPa @Temperature 120 °C | 7830 psi @Temperature 248 °F |
| 54.0 MPa @Temperature 80.0 °C | 7830 psi @Temperature 176 °F |
| 54.0 MPa @Temperature 23.0 °C | 7830 psi @Temperature 73.4 °F |
| 55.2 MPa @Temperature 45.0 °C | 8010 psi @Temperature 113 °F |
| 55.2 MPa @Temperature 23.0 °C | 8010 psi @Temperature 73.4 °F |
| 55.2 MPa @Temperature 23.0 °C | 8010 psi @Temperature 73.4 °F |
| 56.4 MPa @Temperature 23.0 °C | 8180 psi @Temperature 73.4 °F |
| 57.0 MPa @Temperature 23.0 °C | 8270 psi @Temperature 73.4 °F |
| 57.6 MPa @Temperature 23.0 °C | 8350 psi @Temperature 73.4 °F |
| 57.6 MPa @Temperature 23.0 °C | 8350 psi @Temperature 73.4 °F |
| 63.6 MPa @Temperature 120 °C | 9220 psi @Temperature 248 °F |
| 63.6 MPa @Temperature 80.0 °C | 9220 psi @Temperature 176 °F |
| 64.8 MPa @Temperature 45.0 °C | 9400 psi @Temperature 113 °F |
| 65.4 MPa @Temperature 45.0 °C | 9490 psi @Temperature 113 °F |
| 66.0 MPa @Temperature 120 °C | 9570 psi @Temperature 248 °F |
| 66.0 MPa @Temperature 80.0 °C | 9570 psi @Temperature 176 °F |
| 66.6 MPa @Temperature 45.0 °C | 9660 psi @Temperature 113 °F |
| 68.4 MPa @Temperature 80.0 °C | 9920 psi @Temperature 176 °F |
| 69.0 MPa @Temperature 80.0 °C | 10000 psi @Temperature 176 °F |
| 72.6 MPa @Temperature 80.0 °C | 10500 psi @Temperature 176 °F |
| 72.6 MPa @Temperature 80.0 °C | 10500 psi @Temperature 176 °F |
Elongation at Break | >= 300 % | >= 300 % |
Tensile Modulus | 1.40 GPa | 203 ksi |
Flexural Strength | 60.0 MPa | 8700 psi |
Flexural Modulus | 1.60 GPa | 232 ksi |
Charpy Impact Unnotched | NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
| NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
Charpy Impact, Notched | 0.450 J/cm² @Temperature -30.0 °C | 2.14 ft-lb/in² @Temperature -22.0 °F |
| 1.50 J/cm² @Temperature 23.0 °C | 7.14 ft-lb/in² @Temperature 73.4 °F |
Coefficient of Friction, Dynamic | 0.52 | 0.52 |
K (wear) Factor | 34.0 x 10-8 mm³/N-M | 16.9 x 10-10 in³-min/ft-lb-hr |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+13 ohm-cm | 1.00e+13 ohm-cm |
Surface Resistance | 1.00e+13 ohm | 1.00e+13 ohm |
|
Thermal Properties | Metric | English | Comments |
---|
Melting Point | 220 °C | 428 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 85.0 °C | 185 °F |
Flammability, UL94 | HB @Thickness 1.60 mm | HB @Thickness 0.0630 in |
|
Processing Properties | Metric | English | Comments |
---|
Feed Temperature | 60.0 - 80.0 °C | 140 - 176 °F |
Nozzle Temperature | 230 - 250 °C | 446 - 482 °F |
Zone 1 | 210 - 250 °C | 410 - 482 °F |
Zone 2 | 210 - 250 °C | 410 - 482 °F |
Zone 3 | 210 - 250 °C | 410 - 482 °F |
Zone 4 | 210 - 250 °C | 410 - 482 °F |
Melt Temperature | 230 - 250 °C | 446 - 482 °F |
Mold Temperature | 60.0 - 80.0 °C | 140 - 176 °F |
Drying Temperature | 60.0 - 80.0 °C | 140 - 176 °F |
Dry Time | <= 4.00 hour | <= 4.00 hour |
Back Pressure | 30.0 - 80.0 MPa | 4350 - 11600 psi |
|
Descriptive Properties |
---|
Resistance to Acetic Acid | 1% Change in Volume |
| 1% Change in Volume |
| 3% Change in Weight |
| 3% Change in Weight |
Resistance to Acetone | 2% Change in Volume |
| 5% Change in Volume |
| 5% Change in Weight |
| 5% Change in Weight |
Resistance to Ammonium hydroxide 10% | 0% Change in Volume |
| 0% Change in Weight |
| -3% Change in Volume |
| -5% Change in Weight |
Resistance to Antifreeze 50%, 50% water | 0% Change in Volume |
| 0% Change in Weight |
| 1% Change in Volume |
| 1% Change in Weight |
Resistance to Antifreeze, 100% ethylene glycol | 0% Change in Volume |
| 0% Change in Weight |
| 5% Change in Volume |
| 5% Change in Weight |
Resistance to Automatic transmission fluid | 0% Change in Volume |
| 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
Resistance to Brake fluid | 0% Change in Volume |
| 0% Change in Weight |
| 5% Change in Volume |
| 5% Change in Weight |
Resistance to Butyl acetate | 0% Change in Volume |
| 0% Change in Weight |
| 2% Change in Volume |
| 2% Change in Weight |
Resistance to Calcium Chloride | 0% Change in Volume |
| 0% Change in Weight |
Resistance to Chassis lube | 0% Change in Volume |
| 0% Change in Weight |
| -1% Change in Volume |
| -1% Change in Weight |
Resistance to Dichloroethane | 0% Change in Volume |
| 0% Change in Weight |
Resistance to Dimethyl formamide | 0% Change in Volume |
| 2% Change in Weight |
| Samples swell and slowly dissolve |
| Samples swell and slowly dissolve |
Resistance to Ethanol | 1% Change in Volume |
| 2% Change in Volume |
| 2% Change in Weight |
| 2% Change in Weight |
Resistance to Gasohol (unleaded, 10% methanol) | 0% Change in Volume |
| 1% Change in Weight |
| 3% Change in Weight |
| 5% Change in Volume |
Resistance to Gasohol M-25 (unleaded, 15% methanol) | 0% Change in Volume |
| 1% Change in Weight |
| 3% Change in Volume |
| 5% Change in Weight |
Resistance to Heptane | 0% Change in Volume |
| 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
Resistance to Hydraulic fluid | 0% Change in Volume |
| 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
Resistance to Hydrochloric acid | 0% change in volume |
| 0% change in volume |
| 2% change in weight |
| 2% change in weight |
Resistance to Jet fuel A | 0% Change in Volume |
| 0% Change in Weight |
| 1% Change in Weight |
| 2% Change in Volume |
Resistance to Methanol | 1% Change in Volume |
| 2% Change in Weight |
| 2% Change in Weight |
| 3% Change in Volume |
Resistance to Methylethylketone | 2% Change in Volume |
| 2% Change in Weight |
Resistance to Motor oil (SAE 10W-40) | 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
| -1% Change in Volume |
Resistance to MTBE | 1% Change in Volume |
| 1% Change in Weight |
Resistance to Sodium Chloride 10% | 0% Change in Volume |
| 0% Change in Weight |
| 0% Change in Weight |
| -1% Change in Volume |
Resistance to Sodium hydroxide 10% | 0% Change in Volume |
| 1% Change in Weight |
| 5% Change in Volume |
| 5% Change in Weight |
Resistance to Sodium hypochlorite 4.6% | -1% Change in Volume |
| -1% Change in Volume |
| -1% Change in Weight |
| -2% Change in Weight |
Resistance to Sulfuric acid | 0% change in volume |
| 0% change in volume |
| 0% change in weight |
| -1% change in volume |
| -1% change in volume |
| 1% change in weight |
| -1% change in weight |
| -1% change in weight |
Resistance to Tetrachloroethylene | 0% Change in Volume |
| 1% Change in Weight |
| 2% Change in Volume |
| 3% Change in Weight |
Resistance to Toluene | 0% Change in Volume |
| 1% Change in Volume |
| 1% Change in Weight |
| 4% Change in Weight |
Resistance to Trichlorethane | 0% Change in Volume |
| 1% Change in Volume |
| 1% Change in Weight |
| 5% Change in Weight |
Resistance to Unleaded gasoline | 0% Change in Volume |
| 0% Change in Weight |
| 1% Change in Weight |
| 3% Change in Volume |
Resistance to Xylene | 0% Change in Volume |
| 0% Change in Weight |
Resistance to Zinc chloride 10% | 2% Change in Weight |
| 3% Change in Volume |