Physical Properties | Metric | English | Comments |
---|
Density | 9.13 g/cc | 0.330 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 1260 MPa | 183000 psi |
| 285 MPa @Temperature 980 °C | 41300 psi @Temperature 1800 °F |
| 740 MPa @Temperature 760 °C | 107000 psi @Temperature 1400 °F |
| 945 MPa @Temperature 650 °C | 137000 psi @Temperature 1200 °F |
| 1075 MPa @Temperature 540 °C | 155900 psi @Temperature 1000 °F |
Tensile Strength, Yield | 970 MPa @Strain 0.2 % | 141000 psi @Strain 0.2 % |
| 205 MPa @Strain 0.2 %, Temperature 980 °C | 29700 psi @Strain 0.2 %, Temperature 1800 °F |
| 660 MPa @Strain 0.2 %, Temperature 760 °C | 95700 psi @Strain 0.2 %, Temperature 1400 °F |
| 825 MPa @Strain 0.2 %, Temperature 650 °C | 120000 psi @Strain 0.2 %, Temperature 1200 °F |
| 915 MPa @Strain 0.2 %, Temperature 540 °C | 133000 psi @Strain 0.2 %, Temperature 1000 °F |
Elongation at Break | 19 % | 19 % |
| 2.0 % @Temperature 650 °C | 2.0 % @Temperature 1200 °F |
| 3.0 % @Temperature 760 °C | 3.0 % @Temperature 1400 °F |
| 4.0 % @Temperature 980 °C | 4.0 % @Temperature 1800 °F |
| 18 % @Temperature 540 °C | 18 % @Temperature 1000 °F |
Reduction of Area | 19 % | 19 % |
| 2.0 % @Temperature 650 °C | 2.0 % @Temperature 1200 °F |
| 3.0 % @Temperature 760 °C | 3.0 % @Temperature 1400 °F |
| 4.0 % @Temperature 980 °C | 4.0 % @Temperature 1800 °F |
| 18 % @Temperature 540 °C | 18 % @Temperature 1000 °F |
Modulus of Elasticity | 225 GPa | 32600 ksi |
| 146 GPa @Temperature 1000 °C | 21200 ksi @Temperature 1830 °F |
| 154 GPa @Temperature 900 °C | 22300 ksi @Temperature 1650 °F |
| 163 GPa @Temperature 800 °C | 23600 ksi @Temperature 1470 °F |
| 174 GPa @Temperature 700 °C | 25200 ksi @Temperature 1290 °F |
| 181 GPa @Temperature 600 °C | 26300 ksi @Temperature 1110 °F |
| 188 GPa @Temperature 500 °C | 27300 ksi @Temperature 932 °F |
| 197 GPa @Temperature 400 °C | 28600 ksi @Temperature 752 °F |
| 204 GPa @Temperature 300 °C | 29600 ksi @Temperature 572 °F |
| 214 GPa @Temperature 200 °C | 31000 ksi @Temperature 392 °F |
| 222 GPa @Temperature 100 °C | 32200 ksi @Temperature 212 °F |
Charpy Impact | 262 J | 193 ft-lb |
| 144 J @Temperature 980 °C | 106 ft-lb @Temperature 1800 °F |
| 148 J @Temperature -196 °C | 109 ft-lb @Temperature -321 °F |
| 163 J @Temperature 870 °C | 120 ft-lb @Temperature 1600 °F |
| 182 J @Temperature -138 °C | 134 ft-lb @Temperature -216 °F |
| 194 J @Temperature 760 °C | 143 ft-lb @Temperature 1400 °F |
| 212 J @Temperature -78.0 °C | 156 ft-lb @Temperature -108 °F |
| 230 J @Temperature 650 °C | 170 ft-lb @Temperature 1200 °F |
| 243 J @Temperature -29.0 °C | 179 ft-lb @Temperature -20.2 °F |
| 273 J @Temperature 540 °C | 201 ft-lb @Temperature 1000 °F |
| 297 J @Temperature 260 °C | 219 ft-lb @Temperature 500 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000886 ohm-cm | 0.0000886 ohm-cm |
| 0.0000950 ohm-cm @Temperature 1000 °C | 0.0000950 ohm-cm @Temperature 1830 °F |
| 0.0001011 ohm-cm @Temperature 900 °C | 0.0001011 ohm-cm @Temperature 1650 °F |
| 0.0001066 ohm-cm @Temperature 700 °C | 0.0001066 ohm-cm @Temperature 1290 °F |
| 0.0001078 ohm-cm @Temperature 800 °C | 0.0001078 ohm-cm @Temperature 1470 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.3 µm/m-°C @Temperature 25.0 - 100 °C | 6.83 µin/in-°F @Temperature 77.0 - 212 °F |
| 12.9 µm/m-°C @Temperature 25.0 - 200 °C | 7.17 µin/in-°F @Temperature 77.0 - 392 °F |
| 13.6 µm/m-°C @Temperature 25.0 - 300 °C | 7.56 µin/in-°F @Temperature 77.0 - 572 °F |
| 14.3 µm/m-°C @Temperature 25.0 - 500 °C | 7.94 µin/in-°F @Temperature 77.0 - 932 °F |
| 14.3 µm/m-°C @Temperature 25.0 - 400 °C | 7.94 µin/in-°F @Temperature 77.0 - 752 °F |
| 14.6 µm/m-°C @Temperature 25.0 - 600 °C | 8.11 µin/in-°F @Temperature 77.0 - 1110 °F |
| 15.1 µm/m-°C @Temperature 25.0 - 700 °C | 8.39 µin/in-°F @Temperature 77.0 - 1290 °F |
| 15.8 µm/m-°C @Temperature 25.0 - 800 °C | 8.78 µin/in-°F @Temperature 77.0 - 1470 °F |
| 16.5 µm/m-°C @Temperature 25.0 - 900 °C | 9.17 µin/in-°F @Temperature 77.0 - 1650 °F |
| 17.0 µm/m-°C @Temperature 25.0 - 1000 °C | 9.44 µin/in-°F @Temperature 77.0 - 1830 °F |
Thermal Conductivity | 9.40 W/m-K | 65.2 BTU-in/hr-ft²-°F |
| 10.9 W/m-K @Temperature 100 °C | 75.6 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 12.9 W/m-K @Temperature 200 °C | 89.5 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 14.8 W/m-K @Temperature 300 °C | 103 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 16.8 W/m-K @Temperature 400 °C | 117 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 18.7 W/m-K @Temperature 500 °C | 130 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 20.7 W/m-K @Temperature 600 °C | 144 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 22.6 W/m-K @Temperature 700 °C | 157 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 24.7 W/m-K @Temperature 800 °C | 171 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 26.7 W/m-K @Temperature 900 °C | 185 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 29.2 W/m-K @Temperature 1000 °C | 203 BTU-in/hr-ft²-°F @Temperature 1830 °F |
Melting Point | 1330 - 1410 °C | 2430 - 2570 °F |
Solidus | 1330 °C | 2430 °F |
Liquidus | 1410 °C | 2570 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.10 % | 0.10 % |
Chromium, Cr | 20 % | 20 % |
Cobalt, Co | 51 % | 51 % |
Iron, Fe | <= 3.0 % | <= 3.0 % |
Manganese, Mn | 1.5 % | 1.5 % |
Nickel, Ni | 10 % | 10 % |
Silicon, Si | <= 0.40 % | <= 0.40 % |
Tungsten, W | 15 % | 15 % |