MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

High Strength Modified Copper, UNS C19400, O60 Temper flat products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent hot and cold workability.

Applications: circuit breaker components, contact springs, electrical clamps, electrical springs, electrical terminals, flexible hose, fuse clips, gaskets, gift hollow ware, plug contacts, rivets, and welded condenser tubes.

Test specimen: flat products - 0.64mm thickness.

Key Words: CDA 194, HSM Copper
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.78 g/cc0.317 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 3838
Tensile Strength, Ultimate 310 MPa45000 psi
 >= 203 MPa
@Temperature 315 °C
>= 29400 psi
@Temperature 599 °F
annealed strip
 >= 219 MPa
@Temperature 290 °C
>= 31800 psi
@Temperature 554 °F
annealed strip
 >= 235 MPa
@Temperature 260 °C
>= 34100 psi
@Temperature 500 °F
annealed strip
 >= 253 MPa
@Temperature 230 °C
>= 36700 psi
@Temperature 446 °F
annealed strip
 >= 266 MPa
@Temperature 205 °C
>= 38600 psi
@Temperature 401 °F
annealed strip
 >= 276 MPa
@Temperature 175 °C
>= 40000 psi
@Temperature 347 °F
annealed strip
 >= 289 MPa
@Temperature 150 °C
>= 41900 psi
@Temperature 302 °F
annealed strip
 >= 300 MPa
@Temperature 120 °C
>= 43500 psi
@Temperature 248 °F
annealed strip
 >= 313 MPa
@Temperature 95.0 °C
>= 45400 psi
@Temperature 203 °F
annealed strip
 >= 324 MPa
@Temperature 65.0 °C
>= 47000 psi
@Temperature 149 °F
annealed strip
 >= 341 MPa
@Temperature 23.0 °C
>= 49500 psi
@Temperature 73.4 °F
annealed strip
 475 MPa
@Temperature -196 °C
68900 psi
@Temperature -321 °F
Tensile Strength, Yield 195 MPa28300 psi
 <= 150 MPa
@Strain 0.2 %
<= 21800 psi
@Strain 0.2 %
 >= 116 MPa
@Strain 0.2 %,
Temperature 315 °C
>= 16800 psi
@Strain 0.2 %,
Temperature 599 °F
annealed strip
 >= 123 MPa
@Strain 0.2 %,
Temperature 290 °C
>= 17800 psi
@Strain 0.2 %,
Temperature 554 °F
annealed strip
 >= 127 MPa
@Strain 0.2 %,
Temperature 260 °C
>= 18400 psi
@Strain 0.2 %,
Temperature 500 °F
annealed strip
 >= 131 MPa
@Strain 0.2 %,
Temperature 205 °C
>= 19000 psi
@Strain 0.2 %,
Temperature 401 °F
annealed strip
 >= 131 MPa
@Strain 0.2 %,
Temperature 230 °C
>= 19000 psi
@Strain 0.2 %,
Temperature 446 °F
annealed strip
 >= 135 MPa
@Strain 0.2 %,
Temperature 175 °C
>= 19600 psi
@Strain 0.2 %,
Temperature 347 °F
annealed strip
 >= 139 MPa
@Strain 0.2 %,
Temperature 150 °C
>= 20200 psi
@Strain 0.2 %,
Temperature 302 °F
annealed strip
 >= 144 MPa
@Strain 0.2 %,
Temperature 65.0 °C
>= 20900 psi
@Strain 0.2 %,
Temperature 149 °F
annealed strip
 >= 144 MPa
@Strain 0.2 %,
Temperature 95.0 °C
>= 20900 psi
@Strain 0.2 %,
Temperature 203 °F
annealed strip
 >= 144 MPa
@Strain 0.2 %,
Temperature 120 °C
>= 20900 psi
@Strain 0.2 %,
Temperature 248 °F
annealed strip
 >= 150 MPa
@Strain 0.2 %,
Temperature 23.0 °C
>= 21800 psi
@Strain 0.2 %,
Temperature 73.4 °F
annealed strip
Elongation at Break >= 29 %>= 29 %In 50 mm
 38 %
@Temperature -196 °C
38 %
@Temperature -321 °F
Creep Strength  >= 74.0 MPa
@Temperature 315 °C
>= 10700 psi
@Temperature 599 °F
annealed strip
 >= 84.0 MPa
@Temperature 290 °C
>= 12200 psi
@Temperature 554 °F
annealed strip
 >= 96.0 MPa
@Temperature 260 °C
>= 13900 psi
@Temperature 500 °F
annealed strip
 >= 110 MPa
@Temperature 230 °C
>= 16000 psi
@Temperature 446 °F
annealed strip
 >= 124 MPa
@Temperature 205 °C
>= 18000 psi
@Temperature 401 °F
annealed strip
 >= 143 MPa
@Temperature 175 °C
>= 20700 psi
@Temperature 347 °F
annealed strip
 >= 171 MPa
@Temperature 150 °C
>= 24800 psi
@Temperature 302 °F
annealed strip
 >= 190 MPa
@Temperature 120 °C
>= 27600 psi
@Temperature 248 °F
annealed strip
Rupture Strength  >= 47.0 MPa
@Temperature 315 °C
>= 6820 psi
@Temperature 599 °F
annealed strip
 >= 65.0 MPa
@Temperature 290 °C
>= 9430 psi
@Temperature 554 °F
annealed strip
 >= 82.0 MPa
@Temperature 260 °C
>= 11900 psi
@Temperature 500 °F
annealed strip
 >= 105 MPa
@Temperature 230 °C
>= 15200 psi
@Temperature 446 °F
annealed strip
 >= 125 MPa
@Temperature 205 °C
>= 18100 psi
@Temperature 401 °F
annealed strip
 >= 148 MPa
@Temperature 175 °C
>= 21500 psi
@Temperature 347 °F
annealed strip
 >= 171 MPa
@Temperature 150 °C
>= 24800 psi
@Temperature 302 °F
annealed strip
Modulus of Elasticity 121 GPa17500 ksi
Poissons Ratio 0.330.33
Fatigue Strength 110 MPa
@# of Cycles 1.00e+8
16000 psi
@# of Cycles 1.00e+8
rotating beam test
Machinability 20 %20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 65 %65 %
Shear Modulus 45.5 GPa6600 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000431 ohm-cm
@Temperature 20.0 °C
0.00000431 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 16.3 µm/m-°C
@Temperature 20.0 - 300 °C
9.06 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.385 J/g-°C0.0920 BTU/lb-°F
Thermal Conductivity 260 W/m-K
@Temperature 20.0 °C
1800 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1080 - 1090 °C1980 - 1990 °F
Solidus 1080 °C1980 °F
Liquidus 1090 °C1990 °F
Annealing Point 371 - 649 °C700 - 1200 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 97.5 %97.5 %
Iron, Fe 2.1 - 2.6 %2.1 - 2.6 %
Lead, Pb <= 0.030 %<= 0.030 %
Other, total <= 0.15 %<= 0.15 %
Phosphorus, P 0.015 - 0.15 %0.015 - 0.15 %
Tin, Sn <= 0.030 %<= 0.030 %
Zinc, Zn 0.050 - 0.20 %0.050 - 0.20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
High Strength Modified Copper, UNS C19400, O50 Temper flat products
Copper, UNS C19500, H02 Temper
Copper, UNS C19500, H08 Temper
Copper, UNS C19500, O61 Temper
Copper, UNS C19500, O50 Temper

MC19400b3 / 10944

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.