Envalior Durethan® AKV 35 H2.0 901510 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Conditioned
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, 40% Glass Fiber Filled
Material Notes:
PA 66, 35% glass fibers, injection molding, heat-aging stabilized
Former Lanxess product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.41
g/cc
0.0509
lb/in³
ISO 1183
Moisture Absorption at Equilibrium
1.7 %
1.7 %
50% RH; ISO 62
Water Absorption at Saturation
5.0 %
5.0 %
ISO 62
Linear Mold Shrinkage, Flow
0.0037
cm/cm
0.0037
in/in
60x60x2; 300 °C / MT 80°C; 600 bar; ISO 294-4
Linear Mold Shrinkage, Transverse
0.0091
cm/cm
0.0091
in/in
60x60x2; 300 °C / MT 80°C; 600 bar; ISO 294-4
Mechanical Properties
Metric
English
Comments
Puncture Resistance
1260
N
@Temperature 23.0 °C
283
lb (f)
@Temperature 73.4 °F
ISO 6603-2
Ball Indentation Hardness
140
MPa
20300
psi
ISO 2093-1
Tensile Strength at Break
125
MPa
18100
psi
5 mm/min; ISO 527-1,-2
Elongation at Break
6.4 %
6.4 %
5 mm/min; ISO 527-1,-2
Tensile Modulus
7.50
GPa
1090
ksi
1 mm/min; ISO 527-1,-2
Flexural Strength
200
MPa
29000
psi
2 mm/min; ISO 178-A
Flexural Yield Strength
165
MPa
@Strain 3.5 %
23900
psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus
6.50
GPa
943
ksi
2 mm/min; ISO 178-A
Flexural Strain at Break
6.2 %
6.2 %
2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)
10.0
kJ/m²
@Temperature -30.0 °C
4.76
ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
15.0
kJ/m²
@Temperature 23.0 °C
7.14
ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Charpy Impact Unnotched
7.50
J/cm²
@Temperature -30.0 °C
35.7
ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eU
9.00
J/cm²
@Temperature 23.0 °C
42.8
ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eU
Charpy Impact, Notched
1.00
J/cm²
@Temperature -30.0 °C
4.76
ft-lb/in²
@Temperature -22.0 °F
ISO 179 1eA
1.70
J/cm²
@Temperature 23.0 °C
8.09
ft-lb/in²
@Temperature 73.4 °F
ISO 179 1eA
Puncture Energy
5.90
J
@Temperature 23.0 °C
4.35
ft-lb
@Temperature 73.4 °F
ISO 6603-2
Tensile Creep Modulus, 1 hour
7000
MPa
1.02e+6
psi
ISO 899-1
Tensile Creep Modulus, 1000 hours
5800
MPa
841000
psi
ISO 899-1
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+10
ohm-cm
1.00e+10
ohm-cm
IEC 60093
Surface Resistance
1.00e+13
ohm
1.00e+13
ohm
IEC 60093
Dielectric Constant
4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
IEC 60250
10
@Frequency 100 Hz
10
@Frequency 100 Hz
IEC 60250
Dielectric Strength
30.0
kV/mm
@Thickness 1.00 mm
762
kV/in
@Thickness 0.0394 in
IEC 60243-1
Dissipation Factor
0.21
@Frequency 100 Hz
0.21
@Frequency 100 Hz
IEC 60250
0.65
@Frequency 1e+6 Hz
0.65
@Frequency 1e+6 Hz
IEC 60250
Thermal Properties
Metric
English
Comments
Melting Point
263
°C
505
°F
10°C/min; ISO 11357-1,-3
Processing Properties
Metric
English
Comments
Melt Temperature
290
°C
554
°F
injection molding; ISO 294
280
-
300
°C
536
-
572
°F
Mold Temperature
80.0
°C
176
°F
injection molding; ISO 294
80.0
-
120
°C
176
-
248
°F
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Envalior Durethan® AKV 35 H2.0 901510 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Dry
Envalior Durethan® AKV 35 H2.0 SR1 901510 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Dry
Envalior Durethan® AKV 35 H2.0 SR1 901510 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Conditioned
Envalior Durethan® AKV 35 CX H2.0 900876 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Dry
Envalior Durethan® AKV 35 000000 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Dry
PLANW9237 / 208034
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.