MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Menzolit Menzolit® HPC 1200 Unsaturated Polyester UP
Categories: Polymer; Thermoset; Polyester, TS; Thermoset Polyester Glass Filled BMC

Material Notes: HPC 1200 is a special SMC for high strength applications. The glass level has been selected to combine mouldability with high strength and stiffness properties in orientation direction. The reinforcement is composed of chopped, randomly distributed glass fibers and additional unchopped, continuous and lengthwise oriented glass fibers. This results in high strength and stiffness along with the unidirectional fibers. The flowability in orientation direction is reduced. This orientation influences flow during moulding and the anisotropic material properties have to be kept in mind during part design and part moulding. Typical applications are load bearing components, for instance bumpers and power train substructures.

Information Provided by Menzolit

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.80 g/cc0.0650 lb/in³ISO 1183
Water Absorption <= 0.50 %<= 0.50 %ISO 62
Linear Mold Shrinkage -0.000300 cm/cm-0.000300 in/inISO 2577
Linear Mold Shrinkage, Transverse 0.0025 cm/cm0.0025 in/inISO 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 298 MPa
@Temperature 22.0 °C
43200 psi
@Temperature 71.6 °F
25 mm flat samples, compression molded; ISO 527-4
Tensile Strength, Yield 298 MPa
@Temperature 22.0 °C
43200 psi
@Temperature 71.6 °F
25 mm flat samples, compression molded; ISO 527-4
Elongation at Break 1.6 %1.6 %ISO 527-4
Modulus of Elasticity 22.0 GPa3190 ksi25 mm flat samples, compression molded; ISO 527-4
Flexural Strength 655 MPa
@Temperature 22.0 °C
95000 psi
@Temperature 71.6 °F
25 mm wide 100 mm long, flat samples; ISO 14125
Flexural Modulus 24.0 GPa
@Temperature 22.0 °C
3480 ksi
@Temperature 71.6 °F
25 mm wide 100 mm long, flat samples; ISO 14125
Compressive Yield Strength 350 MPa50800 psiISO 14126
Poissons Ratio 0.300.30
Shear Modulus 8.46 GPa1230 ksiCalculated
Charpy Impact, Notched 25.7 J/cm²122 ft-lb/in²ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+12 ohm1.00e+12 ohmIEC 60093
Dielectric Constant 4.04.0IEC 60250
Dielectric Strength 24.0 kV/mm610 kV/inIEC 60243-1
Dissipation Factor 0.0100.010IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.00 µm/m-°C3.89 µin/in-°FISO 11359-2
Specific Heat Capacity 1.10 J/g-°C0.263 BTU/lb-°F
Thermal Conductivity 0.700 W/m-K4.86 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 170 °C338 °F
Deflection Temperature at 1.8 MPa (264 psi) >= 200 °C>= 392 °FISO 75-2
Minimum Service Temperature, Air -40.0 °C-40.0 °F
Glass Transition Temp, Tg 162 °C324 °FISO 11357-2
Flammability, UL94 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
Oxygen Index 22 %22 %ISO 4589-2
Glow Wire Flammability Index 750 °C1380 °FIEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Processing Temperature 135 - 150 °C275 - 302 °FCompression molding, matched metal die

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Menzolit Menzolit® HPC 1300 Unsaturated Polyester UP
Menzolit Menzolit® MMC 1600 Unsaturated Polyester UP
Menzolit Menzolit® SMC 0150 Unsaturated Polyester UP
Menzolit Menzolit® SMC 1100 Unsaturated Polyester UP
Menzolit Menzolit® SMC 1400 Unsaturated Polyester UP

PMENZ027 / 100761

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.