MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Park Aerospace Nelcote® F-562 Phenolic Prepreg, 8HS Silica Reinforced
Categories: Polymer; Thermoset; Phenolic

Material Notes: Nelcote® F-562 is an elastomer modified phenolic resin used in the manufacture of intermediate temperature ablative rocket nozzles, heat shields and combustion chambers in highly oxidative environments.

Key Features and Benefits:

  • Provides a combination of high-strength and ablative properties for demanding applications
  • Low thermal expansion
  • Good Tack and Drape properties
  • Highly toughened resin system for improved impact resistance

Applications/Qualifications:

  • Rocket Nozzles
  • Combustion Chambers
  • Heat Shields
  • Exhaust Gas Management

Information provided by Park Electrochemical Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Volatiles 1.0 - 3.0 %
@Temperature 135 °C
1.0 - 3.0 %
@Temperature 275 °F
8 min
Thickness 559 microns22.0 milnominal, cured, per ply
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 103 MPa
@Temperature 23.9 °C
15000 psi
@Temperature 75.0 °F
0° Direction, Dry; ASTM D638
Tensile Modulus 17.2 GPa
@Temperature 23.9 °C
2500 ksi
@Temperature 75.0 °F
0° Direction, Dry; ASTM D638
Flexural Strength 186 MPa
@Temperature 23.9 °C
27000 psi
@Temperature 75.0 °F
Dry; ASTM D790
Flexural Modulus 22.8 GPa
@Temperature 23.9 °C
3300 ksi
@Temperature 75.0 °F
Dry; ASTM D790
Compressive Strength 448 MPa
@Temperature 23.9 °C
65000 psi
@Temperature 75.0 °F
Dry; ASTM D695
Compressive Modulus 21.4 GPa
@Temperature 23.9 °C
3100 ksi
@Temperature 75.0 °F
Dry; ASTM D695
 
Processing PropertiesMetricEnglishComments
Shelf Life 6.00 Month
@Temperature 4.44 °C
6.00 Month
@Temperature 40.0 °F
 
Descriptive Properties
Resin Flow (%)1-5260°F, 150psi
Resin Solids Content (%)27-30

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Park Aerospace Nelcote® F-554 Phenolic Prepreg, Aerospace Silica Fabric Reinforced
Park Aerospace Nelcote® F-554 Phenolic Prepreg, Commercial Silica Fabric Reinforced
Park Aerospace Nelcote® F-502 Phenolic Prepreg, Silica Reinforced
Park Aerospace Nelcote® F-557 Phenolic Prepreg, Commercial Silica Fabric Reinforced
Park Aerospace Nelcote® F-557 Phenolic Prepreg, Aerospace Silica Fabric Reinforced

PPARK061 / 89333

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.