MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes Hastelloy® C-4 alloy, welded plate 12.7 mm (1/2 in.) thick, GTAW
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Nickel-chromium-molybdenum alloy with outstanding high-temperature stability as evidenced by high ductility and corrosion resistance even after aging in the 1200 to 1900°F (649 to 1038°C) range. This alloy resists the formation of grain-boundary precipitates in the weld heat-affected zone, thus making it suitable for most chemical process applications in the as-welded condition. C-4 alloy also has excellent resistance to stress-corrosion cracking and to oxidizing atmospheres up to 1900°F (1038°C).

HASTELLOY C-4 alloy has exceptional resistance to wide variety of chemical process environments. These include hot contaminated mineral acids, solvents, chlorine and chlorine contaminated media (organic and inorganic), dry chlorine, formic and acetic acids, acetic anhydride, and seawater and brine solutions. Laboratory precipitation studies on C-4 alloy indicate that the intermetallic precipitates (Mu phase) associated with other nickel alloys in the 1200 to 2000°F (649 to 1093°C) temperature range have not been detected. Fine intergranular M6C carbides can form but their damaging effect is minimal.

HASTELLOY C-4 alloy can be forged, hot-upset, and impact extruded. Although the alloy tends to work-harden, it can be successfully deep-drawn, spun, press formed or punched. All of the common methods of welding can be used to weld HASTELLOY C-4 alloy, although the oxy-acetylene and submerged arc processes are not recommended when the fabricated item is intended for use in corrosion service. Special precautions should be taken to avoid excessive heat input.

Wrought forms of HASTELLOY C-4 alloy are furnished in the solution heat-treated condition unless otherwise specified. C-4 alloy is solution heat-treated at 1950°F (1066°C) and rapid quenched.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N06455; ASME SB-574, ASME SB-575, ASME SB-6119, SB-622 and ASME SB-626
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.64 g/cc0.312 lb/in³at RT
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 777 MPa113000 psi
 602 MPa
@Temperature 538 °C
87300 psi
@Temperature 1000 °F
 654 MPa
@Temperature 260 °C
94900 psi
@Temperature 500 °F
Tensile Strength, Yield 471 MPa
@Strain 0.2 %
68300 psi
@Strain 0.2 %
 336 MPa
@Strain 0.2 %,
Temperature 538 °C
48700 psi
@Strain 0.2 %,
Temperature 1000 °F
 352 MPa
@Strain 0.2 %,
Temperature 260 °C
51100 psi
@Strain 0.2 %,
Temperature 500 °F
Elongation at Break 40 %40 %in 50.8 mm
 35 %
@Temperature 538 °C
35 %
@Temperature 1000 °F
in 50.8 mm
 39 %
@Temperature 260 °C
39 %
@Temperature 500 °F
in 50.8 mm
Modulus of Elasticity 211 GPa30600 ksiRT
 141 GPa
@Temperature 982 °C
20500 ksi
@Temperature 1800 °F
 152 GPa
@Temperature 871 °C
22000 ksi
@Temperature 1600 °F
 162 GPa
@Temperature 760 °C
23500 ksi
@Temperature 1400 °F
 171 GPa
@Temperature 649 °C
24800 ksi
@Temperature 1200 °F
 179 GPa
@Temperature 538 °C
26000 ksi
@Temperature 1000 °F
 187 GPa
@Temperature 427 °C
27100 ksi
@Temperature 801 °F
 194 GPa
@Temperature 316 °C
28100 ksi
@Temperature 601 °F
 201 GPa
@Temperature 204 °C
29200 ksi
@Temperature 399 °F
 207 GPa
@Temperature 93.0 °C
30000 ksi
@Temperature 199 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.000125 ohm-cm
@Temperature 23.0 °C
0.000125 ohm-cm
@Temperature 73.4 °F
 0.000125 ohm-cm
@Temperature 100 °C
0.000125 ohm-cm
@Temperature 212 °F
 0.000126 ohm-cm
@Temperature 200 °C
0.000126 ohm-cm
@Temperature 392 °F
 0.000127 ohm-cm
@Temperature 300 °C
0.000127 ohm-cm
@Temperature 572 °F
 0.000128 ohm-cm
@Temperature 400 °C
0.000128 ohm-cm
@Temperature 752 °F
 0.000129 ohm-cm
@Temperature 500 °C
0.000129 ohm-cm
@Temperature 932 °F
 0.000132 ohm-cm
@Temperature 600 °C
0.000132 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.8 µm/m-°C
@Temperature 20.0 - 93.0 °C
6.00 µin/in-°F
@Temperature 68.0 - 199 °F
 11.9 µm/m-°C
@Temperature 20.0 - 204 °C
6.61 µin/in-°F
@Temperature 68.0 - 399 °F
 12.6 µm/m-°C
@Temperature 20.0 - 316 °C
7.00 µin/in-°F
@Temperature 68.0 - 601 °F
 13.3 µm/m-°C
@Temperature 20.0 - 427 °C
7.39 µin/in-°F
@Temperature 68.0 - 801 °F
 13.3 µm/m-°C
@Temperature 20.0 - 538 °C
7.39 µin/in-°F
@Temperature 68.0 - 1000 °F
 13.5 µm/m-°C
@Temperature 20.0 - 649 °C
7.50 µin/in-°F
@Temperature 68.0 - 1200 °F
 14.4 µm/m-°C
@Temperature 20.0 - 760 °C
8.00 µin/in-°F
@Temperature 68.0 - 1400 °F
 14.9 µm/m-°C
@Temperature 24.0 - 871 °C
8.28 µin/in-°F
@Temperature 75.2 - 1600 °F
 15.7 µm/m-°C
@Temperature 20.0 - 982 °C
8.72 µin/in-°F
@Temperature 68.0 - 1800 °F
Specific Heat Capacity  0.406 J/g-°C
@Temperature 0.000 °C
0.0970 BTU/lb-°F
@Temperature 32.0 °F
 0.427 J/g-°C
@Temperature 100 °C
0.102 BTU/lb-°F
@Temperature 212 °F
 0.448 J/g-°C
@Temperature 200 °C
0.107 BTU/lb-°F
@Temperature 392 °F
 0.465 J/g-°C
@Temperature 300 °C
0.111 BTU/lb-°F
@Temperature 572 °F
 0.477 J/g-°C
@Temperature 400 °C
0.114 BTU/lb-°F
@Temperature 752 °F
 0.490 J/g-°C
@Temperature 500 °C
0.117 BTU/lb-°F
@Temperature 932 °F
 0.502 J/g-°C
@Temperature 600 °C
0.120 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity  10.1 W/m-K
@Temperature 23.0 °C
70.1 BTU-in/hr-ft²-°F
@Temperature 73.4 °F
 11.4 W/m-K
@Temperature 100 °C
79.1 BTU-in/hr-ft²-°F
@Temperature 212 °F
 13.2 W/m-K
@Temperature 200 °C
91.6 BTU-in/hr-ft²-°F
@Temperature 392 °F
 15.0 W/m-K
@Temperature 300 °C
104 BTU-in/hr-ft²-°F
@Temperature 572 °F
 16.7 W/m-K
@Temperature 400 °C
116 BTU-in/hr-ft²-°F
@Temperature 752 °F
 18.4 W/m-K
@Temperature 500 °C
128 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.5 W/m-K
@Temperature 600 °C
142 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.010 %<= 0.010 %
Chromium, Cr 14 - 18 %14 - 18 %
Cobalt, Co <= 2.0 %<= 2.0 %
Iron, Fe <= 3.0 %<= 3.0 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 14 - 17 %14 - 17 %
Nickel, Ni 58 %58 %As Remainder
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si <= 0.080 %<= 0.080 %
Sulfur, S <= 0.010 %<= 0.010 %
Titanium, Ti <= 0.70 %<= 0.70 %
 
Descriptive Properties
Average Oxidation Rate per 100-hour test period (mm)0.004at 1038°C
Thermal Diffusivity0.028 cm2/sat 23°C
 0.031 cm2/sat 100°C
 0.033 cm2/sat 200°C
 0.037 cm2/sat 300°C
 0.04 cm2/sat 400°C
 0.043 cm2/sat 500°C
 0.047 cm2/sat 600°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Haynes Hastelloy® C-4 alloy, sheet, aged 100 hours at 899°C
Haynes Hastelloy® C-4 alloy, sheet, heat treated at 1066°C, rapid quenched
Haynes Hastelloy® C-4 alloy, plate, heat treated at 1066°C, rapid quenched
MetalTek MTEK CW-2M Cast UNS N26455 Severe Corrosion and Heat Resistant Alloy
Haynes Hastelloy® C-4 alloy, welded plate 12.7 mm (1/2 in.) thick, aged 10 hours at 649°C (1200°F)

NHC4BU / 17196

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.