Envalior Stanyl® TW272B6 (PA46+PTFE)-CF30, Dry, 30% Carbon Fiber, Heat Stabilized
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 46 (PA46)
Material Notes:
30% Carbon Reinforced, Heat Stabilized, Wear and Friction Modified
Former DSM Engineering Plastics product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.35
g/cc
0.0488
lb/in³
ISO 1183
Moisture Absorption
2.25 %
2.25 %
Humidity; Sim. ISO 62
Linear Mold Shrinkage, Flow
0.0030
cm/cm
0.0030
in/in
ISO 294-4
Linear Mold Shrinkage, Transverse
0.0060
cm/cm
0.0060
in/in
ISO 294-4
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
240
MPa
34800
psi
ISO 527-1/-2
90.0
MPa
@Temperature 200 °C
13100
psi
@Temperature 392 °F
ISO 527-1/-2
100
MPa
@Temperature 180 °C
14500
psi
@Temperature 356 °F
ISO 527-1/-2
110
MPa
@Temperature 160 °C
16000
psi
@Temperature 320 °F
ISO 527-1/-2
130
MPa
@Temperature 120 °C
18900
psi
@Temperature 248 °F
ISO 527-1/-2
Elongation at Break
1.6 %
1.6 %
ISO 527-1/-2
3.1 %
@Temperature 120 °C
3.1 %
@Temperature 248 °F
ISO 527-1/-2
3.1 %
@Temperature 160 °C
3.1 %
@Temperature 320 °F
ISO 527-1/-2
3.1 %
@Temperature 180 °C
3.1 %
@Temperature 356 °F
ISO 527-1/-2
3.1 %
@Temperature 200 °C
3.1 %
@Temperature 392 °F
ISO 527-1/-2
Tensile Modulus
24.0
GPa
3480
ksi
ISO 527-1/-2
10.0
GPa
@Temperature 200 °C
1450
ksi
@Temperature 392 °F
ISO 527-1/-2
10.5
GPa
@Temperature 180 °C
1520
ksi
@Temperature 356 °F
ISO 527-1/-2
11.0
GPa
@Temperature 160 °C
1600
ksi
@Temperature 320 °F
ISO 527-1/-2
12.5
GPa
@Temperature 120 °C
1810
ksi
@Temperature 248 °F
ISO 527-1/-2
Charpy Impact Unnotched
5.00
J/cm²
@Temperature 23.0 °C
23.8
ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
5.00
J/cm²
@Temperature -30.0 °C
23.8
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched
0.600
J/cm²
@Temperature 23.0 °C
2.86
ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
0.600
J/cm²
@Temperature -30.0 °C
2.86
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
25.0
µm/m-°C
13.9
µin/in-°F
ISO 11359-1/-2
CTE, linear, Transverse to Flow
35.0
µm/m-°C
19.4
µin/in-°F
ISO 11359-1/-2
Melting Point
295
°C
563
°F
10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi)
290
°C
554
°F
ISO 72-1/-2
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Saint-Gobain Chemfab® 14 High-Performance PTFE-Coated Glass
Envalior Stanyl® TW200B6 PA46-CF30, Dry, 30% Carbon Reinforced, Heat Stabilized
Envalior Stanyl® TW200F8 PA46-GF40, Dry, 40% Glass Filled, Heat Stabilized
Mitsubishi Chemical Advanced Materials Ketron™ CM HPV PEEK Polyetheretherketone; PTFE, Graphite, and Carbon Fiber Filled Bearing Grade, compression molded
Envalior Stanyl® TW200F3 PA46-GF15, Dry, 15% Glass Filled, Heat Stabilized
PDSM8257 / 184958
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.