MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ovako S235JR SS 14 13 12:1987 (ref) Steel, +AR
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: Soft structural steel easy to weld and bend.

Information provided by Ovako

Key Words: SS 1312, S235JR, 1.0038, Fe 360 BFN, RSt37-2, 40 B
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  <= 130
@Thickness <=40.0 mm
<= 130
@Thickness <=1.57 in
All formats
 <= 130
@Thickness 40.1 - 100 mm
<= 130
@Thickness 1.58 - 3.94 in
All formats
Tensile Strength  360 - 460 MPa
@Thickness <=40.0 mm
52200 - 66700 psi
@Thickness <=1.57 in
All formats
 360 - 460 MPa
@Thickness 40.1 - 100 mm
52200 - 66700 psi
@Thickness 1.58 - 3.94 in
All formats
Tensile Strength, Yield  >= 230 MPa
@Thickness 40.1 - 100 mm
>= 33400 psi
@Thickness 1.58 - 3.94 in
Reh, All formats
 >= 240 MPa
@Thickness <=40.0 mm
>= 34800 psi
@Thickness <=1.57 in
Reh, All formats
Elongation at Break  25 %
@Thickness <=40.0 mm
25 %
@Thickness <=1.57 in
All formats
 25 %
@Thickness 40.1 - 100 mm
25 %
@Thickness 1.58 - 3.94 in
All formats
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 485 °C905 °FMS
 725 °C1340 °FAC1
 863 °C1590 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.20 %<= 0.20 %
Iron, Fe >= 99.69 %>= 99.69 %As Balance
Nitrogen, N <= 0.012 %<= 0.012 %
Phosphorus, P <= 0.050 %<= 0.050 %
Sulfur, S <= 0.050 %<= 0.050 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ovako S235JR EN10025-2 (ref) Steel, +AR
EN S235JR High Manganese, Structural, Hot Rolled, Base Steel, t < 16 mm
ASTM A284 Steel, grade C
EN S235JR Structural, Hot Rolled, Base Steel, 16 mm < t < 25 mm
ASTM A284 Steel, grade D

NOVAKO409 / 234708

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.