MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel, condition H1150M
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless; T S10000 Series Stainless Steel

Material Notes: Martensitic, precipitative hardening (maraging), combining high strength and hardness with excellent corrosion resistance. Applications include valve parts, fittings and fasteners, shafts, gears, chemical process equipment, paper mill equipment, aircraft components and nuclear reactor components.

Key Words: 15-5 PH, 15-5PH, 15/5 PH, 15/5PH, XM12, AMS 5862, ASME SA705 (XM-12), ASTM A564 (XM-12), ASTM A693 (XM-12), ASTM A705 (XM-12), AFNOR NF A35-581 Z6CNU15.05, DIN 1.4540, DIN X4CrNiCuNb164, Cr-Ni 15-5, UNS S15500, AMS 5658, AMS 5659, AMS 5826
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³Solution treated plus 480°C for 1 hour, air cooled.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 896 MPa130000 psi
 552 MPa
@Temperature 540 °C
80100 psi
@Temperature 1000 °F
 676 MPa
@Temperature 425 °C
98000 psi
@Temperature 797 °F
 717 MPa
@Temperature 315 °C
104000 psi
@Temperature 599 °F
 765 MPa
@Temperature 205 °C
111000 psi
@Temperature 401 °F
 1041 MPa
@Temperature -73.0 °C
151000 psi
@Temperature -99.4 °F
 1386 MPa
@Temperature -195 °C
201000 psi
@Temperature -319 °F
Tensile Strength, Yield 717 MPa
@Strain 0.2 %
104000 psi
@Strain 0.2 %
 462 MPa
@Strain 0.2 %,
Temperature 540 °C
67000 psi
@Strain 0.2 %,
Temperature 1000 °F
 607 MPa
@Strain 0.2 %,
Temperature 425 °C
88000 psi
@Strain 0.2 %,
Temperature 797 °F
 662 MPa
@Strain 0.2 %,
Temperature 315 °C
96000 psi
@Strain 0.2 %,
Temperature 599 °F
 689 MPa
@Strain 0.2 %,
Temperature 205 °C
99900 psi
@Strain 0.2 %,
Temperature 401 °F
 738 MPa
@Strain 0.2 %,
Temperature -73.0 °C
107000 psi
@Strain 0.2 %,
Temperature -99.4 °F
 1007 MPa
@Strain 0.2 %,
Temperature -195 °C
146100 psi
@Strain 0.2 %,
Temperature -319 °F
Elongation at Break 23 %23 %gage length is 4 times diameter
 17 %
@Temperature 425 °C
17 %
@Temperature 797 °F
gage length is 4 times diameter
 19 %
@Temperature 315 °C
19 %
@Temperature 599 °F
gage length is 4 times diameter
 20 %
@Temperature 205 °C
20 %
@Temperature 401 °F
gage length is 4 times diameter
 20 %
@Temperature 540 °C
20 %
@Temperature 1000 °F
gage length is 4 times diameter
 25 %
@Temperature -73.0 °C
25 %
@Temperature -99.4 °F
gage length is 4 times diameter
 27 %
@Temperature -195 °C
27 %
@Temperature -319 °F
gage length is 4 times diameter
Modulus of Elasticity 200 GPa29000 ksiTypical elastic modulus for stainless steel
Charpy Impact 236 J174 ft-lb
 45.0 J
@Temperature -195 °C
33.2 ft-lb
@Temperature -319 °F
 206 J
@Temperature -73.0 °C
152 ft-lb
@Temperature -99.4 °F
 226 J
@Temperature -40.0 °C
167 ft-lb
@Temperature -40.0 °F
 233 J
@Temperature -12.0 °C
172 ft-lb
@Temperature 10.4 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000770 ohm-cm0.0000770 ohm-cmSolution treated plus 480°C for 1 hour, air cooled.
Magnetic Permeability 9595approximate value for the annealed condition at RT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.4 µm/m-°C
@Temperature -73.0 - 21.0 °C
5.78 µin/in-°F
@Temperature -99.4 - 69.8 °F
 10.8 µm/m-°C
@Temperature 21.0 - 205 °C
6.00 µin/in-°F
@Temperature 69.8 - 401 °F
 10.8 µm/m-°C
@Temperature 21.0 - 93.0 °C
6.00 µin/in-°F
@Temperature 69.8 - 199 °F
 11.3 µm/m-°C
@Temperature 21.0 - 315 °C
6.28 µin/in-°F
@Temperature 69.8 - 599 °F
Specific Heat Capacity 0.420 J/g-°C0.100 BTU/lb-°FSolution treated plus 480°C for 1 hour, air cooled.
Thermal Conductivity  17.8 W/m-K
@Temperature 150 °C
124 BTU-in/hr-ft²-°F
@Temperature 302 °F
 19.5 W/m-K
@Temperature 260 °C
135 BTU-in/hr-ft²-°F
@Temperature 500 °F
 22.5 W/m-K
@Temperature 460 °C
156 BTU-in/hr-ft²-°F
@Temperature 860 °F
 22.7 W/m-K
@Temperature 480 °C
158 BTU-in/hr-ft²-°F
@Temperature 896 °F
Melting Point 1405 - 1440 °C2561 - 2620 °F
Solidus 1405 °C2561 °F
Liquidus 1440 °C2620 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.070 %<= 0.070 %
Chromium, Cr 14.8 %14.8 %
Copper, Cu 3.5 %3.5 %
Iron, Fe 75 %75 %
Manganese, Mn <= 1.0 %<= 1.0 %
Nb + Ta 0.30 %0.30 %
Nickel, Ni 4.5 %4.5 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel, condition H1100
AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel, condition H1025
AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel, condition H925
AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel transverse direction, condition H1150
AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel transverse direction, condition H900

MQM15AK / 13523

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.