CENTROPLAST CENTRODAL GF Polyoxymethylene 30% glass fiber
Categories:
Polymer
;
Thermoplastic
;
Acetal (Polyoxymethylene, POM)
;
Acetal Copolymer, 30% Glass Fiber Reinforced
Material Notes:
This material has good hot water resistance and sliding properties. Its applications include seals, scrapers and chain guides, and toothed wheels and rollers.
Information provided by CENTROPLAST Engineering Plastics GMBH
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.60
g/cc
0.0578
lb/in³
ISO 1183
Moisture Absorption at Equilibrium
0.17 %
0.17 %
in normal climate 23°C/50%RH; ISO 62
Water Absorption at Saturation
0.90 %
0.90 %
in water at 23°C; ISO 62
Mechanical Properties
Metric
English
Comments
Ball Indentation Hardness
200
MPa
29000
psi
value at 30 sec.; ISO 2039-1
Tensile Strength, Yield
135
MPa
19600
psi
v = 50 mm/min; ISO 527-2
Elongation at Break
4.0 %
4.0 %
ISO 527-2
Tensile Modulus
9.20
GPa
1330
ksi
ISO 527-2
Flexural Modulus
7.80
GPa
1130
ksi
ISO 178
Charpy Impact Unnotched
3.00
J/cm²
14.3
ft-lb/in²
ISO 179/1eU
Charpy Impact, Notched
0.800
J/cm²
3.81
ft-lb/in²
ISO 179/1eA
Electrical Properties
Metric
English
Comments
Electrical Resistivity
1.00e+15
ohm-cm
1.00e+15
ohm-cm
IEC 60093
Surface Resistance
1.00e+12
ohm
1.00e+12
ohm
IEC 60093
Dielectric Constant
4.3
@Frequency 100 Hz
4.3
@Frequency 100 Hz
IEC 60250
4.3
@Frequency 1e+6 Hz
4.3
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength
40.0
kV/mm
1020
kV/in
in transformer oil; IEC 60243-1
Dissipation Factor
0.0030
@Frequency 100 Hz
0.0030
@Frequency 100 Hz
IEC 60250
0.0060
@Frequency 1e+6 Hz
0.0060
@Frequency 1e+6 Hz
IEC 60250
Thermal Properties
Metric
English
Comments
CTE, linear
40.0
µm/m-°C
@Temperature 20.0 °C
22.2
µin/in-°F
@Temperature 68.0 °F
ISO 11359
Melting Point
166
°C
331
°F
10K/min; ISO 3146
Maximum Service Temperature, Air
100
°C
212
°F
Long Term
140
°C
284
°F
Short term
Deflection Temperature at 1.8 MPa (264 psi)
160
°C
320
°F
ISO 75-2
Vicat Softening Point
158
°C
316
°F
VST/B/50; ISO 306
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
CENTROPLAST CENTRODAL TF Polyoxymethylene + PTFE
Chase Plastics CP Pryme® AH120 Acetal Copolymer, 20% Glass Fiber Reinforced
DuPont Mobility and Materials Delrin® 100AF POM-PTFE20
Barlog Plastics KEBAFORM C 1090 POM Copolymer, 10% glass fiber reinforced
Avient Edgetek® ATH-25GF-10MN/000 Acetal-Homopolymer, Glass/Mineral Filled
PCENTR03 / 27954
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.