MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Plastcom SLOVALEN PH 76 FRD 3 PP, flame retardant  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Flame Retardant

Material Notes: Features

Determined for environment, where contact with water is possible, because the electric properties do not change by conditioning. Application - terminals, coil forms, guides in washing machines, tea-pots, dish-washers. Delivered in natural mode and in the full RAL colour scale. Modified homopolymer PP, retarded type with halogen flame retardant. Fulfills basic electric properties: flammability in accordance with UL 94 V0 and 960°C glow wire.

Packaging, transport, stocking

The product is packed in hermetically closed thick-walled 25 kg PE bags, on a 1.000 kg palette coated in a stretch foil, in big bags with a thick PE foil fixed on a 1.000 kg palette, in paper octabins with a thick PE foil fixed on a 1.000 kg palette or in other packaging according to customer requirements. The transport is provided in closed-up vehicles where the material is protected against movement and mechanical damage. The product requires stocking in closed-up, dry places protected against sun and thermal radiation.

Information Provided by Plastcom spol. s r.o.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0397 lb/in³
Linear Mold Shrinkage 0.0218 cm/cm0.0218 in/in
Linear Mold Shrinkage, Transverse 0.0197 cm/cm0.0197 in/in
Melt Flow 25 g/10 min
@Load 0.325 kg,
Temperature 270 °C
25 g/10 min
@Load 0.716 lb,
Temperature 518 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 30.0 MPa4350 psi
Elongation at Break 10 %10 %
Tensile Modulus 1.30 GPa189 ksi
Flexural Strength 35.0 MPa5080 psi
Flexural Modulus 1.30 GPa189 ksi
Charpy Impact Unnotched  1.50 J/cm²
@Temperature -20.0 °C
7.14 ft-lb/in²
@Temperature -4.00 °F
 9.00 J/cm²
@Temperature 23.0 °C
42.8 ft-lb/in²
@Temperature 73.4 °F
Charpy Impact, Notched  0.100 J/cm²
@Temperature -20.0 °C
0.476 ft-lb/in²
@Temperature -4.00 °F
 0.300 J/cm²
@Temperature 23.0 °C
1.43 ft-lb/in²
@Temperature 73.4 °F
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cm
Surface Resistance 1.00e+16 ohm1.00e+16 ohm
Dielectric Strength 26.0 kV/mm660 kV/in
Comparative Tracking Index 450 V450 V
 
Thermal PropertiesMetricEnglishComments
Melting Point 160 °C320 °F
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °C194 °F
Vicat Softening Point 150 °C302 °FB
Flammability, UL94 V-0V-0
Glow Wire Test 960 °C1760 °F
 
Processing PropertiesMetricEnglishComments
Melt Temperature 200 - 250 °C392 - 482 °F
Mold Temperature 30.0 - 50.0 °C86.0 - 122 °F
Injection Pressure 50.0 - 80.0 MPa7250 - 11600 psi

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Plastcom SLOVALEN PH 78 FRT 5 Polypropylene Homopolymer, Halogen Free and Phosphor Free Flame Retardant
Multibase Multi-Flam™ 0220 PP Polypropylene
Multibase Multi-Flam™ 0206 PP Polypropylene
Multibase Multi-Flam™ 0302 PP NH Polypropylene
Multibase Multi-Flam™ 0501 PP Polypropylene

PPLACO229 / 120853

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.