MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI 8630H Steel, normalized
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 8000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes:

Key Words: UNS H86300, ASTM A304, SAE J1268, DIN 1.6545, UNI 30 NiCrMo 2 KB
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.85 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 230230Converted from Vickers hardness.
 266
@Temperature -79.0 °C
266
@Temperature -110 °F
Converted from Vickers hardness
 305
@Temperature -195 °C
305
@Temperature -319 °F
Converted from Vickers hardness
Hardness, Rockwell C 1515Converted from Vickers hardness. Value below normal HRC range, for comparison only.
 22
@Temperature -79.0 °C
22
@Temperature -110 °F
Converted from Vickers hardness
 28
@Temperature -195 °C
28
@Temperature -319 °F
Converted from Vickers hardness
Hardness, Vickers 217217
 252
@Temperature -79.0 °C
252
@Temperature -110 °F
 289
@Temperature -195 °C
289
@Temperature -319 °F
Tensile Strength, Ultimate 620 MPa89900 psi
 717 MPa
@Temperature -79.0 °C
104000 psi
@Temperature -110 °F
 1035 MPa
@Temperature -195 °C
150100 psi
@Temperature -319 °F
Tensile Strength, Yield 550 MPa
@Strain 0.2 %
79800 psi
@Strain 0.2 %
 635 MPa
@Strain 0.2 %,
Temperature -79.0 °C
92100 psi
@Strain 0.2 %,
Temperature -110 °F
 924 MPa
@Strain 0.2 %,
Temperature -195 °C
134000 psi
@Strain 0.2 %,
Temperature -319 °F
Elongation at Break 16 %16 %in 50 mm
 12 %
@Temperature -195 °C
12 %
@Temperature -319 °F
in 50 mm
 18 %
@Temperature -79.0 °C
18 %
@Temperature -110 °F
in 50 mm
Modulus of Elasticity 187 GPa27100 ksi
 199 GPa
@Temperature -79.0 °C
28900 ksi
@Temperature -110 °F
 220 GPa
@Temperature -195 °C
31900 ksi
@Temperature -319 °F
Bulk Modulus 160 GPa23200 ksiTypical for steel.
Poissons Ratio 0.300.30Calculated
Fatigue Strength 315 MPa45700 psiUnnotched Limit
 400 MPa
@Temperature -79.0 °C
58000 psi
@Temperature -110 °F
Unnotched Limit
 640 MPa
@Temperature -195 °C
92800 psi
@Temperature -319 °F
Unnotched Limit
Machinability 70 %70 %annealed and cold drawn. Based on AISI 1212 steel = 100%.
Shear Modulus 72.0 GPa10400 ksiEstimated from elastic modulus
 76.5 GPa
@Temperature -79.0 °C
11100 ksi
@Temperature -110 °F
Estimated from elastic modulus
 84.6 GPa
@Temperature -195 °C
12300 ksi
@Temperature -319 °F
Estimated from elastic modulus
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000234 ohm-cm0.0000234 ohm-cmTypical steel
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.2 µm/m-°C
@Temperature 21.0 - 100 °C
6.22 µin/in-°F
@Temperature 69.8 - 212 °F
 12.2 µm/m-°C
@Temperature 21.0 - 200 °C
6.78 µin/in-°F
@Temperature 69.8 - 392 °F
 14.0 µm/m-°C
@Temperature 21.0 - 500 °C
7.78 µin/in-°F
@Temperature 69.8 - 932 °F
Specific Heat Capacity 0.475 J/g-°C0.114 BTU/lb-°FTypical steel
Thermal Conductivity 46.6 W/m-K323 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.27 - 0.33 %0.27 - 0.33 %
Chromium, Cr 0.35 - 0.65 %0.35 - 0.65 %
Iron, Fe 96.695 - 98.08 %96.695 - 98.08 %As remainder
Manganese, Mn 0.65 - 0.95 %0.65 - 0.95 %
Molybdenum, Mo 0.15 - 0.25 %0.15 - 0.25 %
Nickel, Ni 0.35 - 0.75 %0.35 - 0.75 %
Phosphorus, P <= 0.035 %<= 0.035 %
Silicon, Si 0.15 - 0.30 %0.15 - 0.30 %
Sulfur, S <= 0.040 %<= 0.040 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 8630 Steel, normalized
AISI 1020 Steel, normalized at 870°C (1600°F)
AISI 8630 Steel, water quenched 845°C (1550°F), 480°C (900°F) temper, 100 mm (4 in.) round
AISI 8630 Steel, water quenched 845°C (1550°F), 480°C (900°F) temper, 50 mm (2 in.) round
AISI 1144 Steel, normalized at 900°C (1650°F)

M863BA / 8407

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.