MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Braskem Green PE SLL5405S Blown Film Extrusion High Density Polyethylene
Categories: Polymer; Film; Renewable/Recycled Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Blow Molding Grade

Material Notes: Description: SLL5405S is a LLDPE Butene copolymer produced by Braskem. It is a general purpose product that shows a good processing performance balanced with good mechanical properties as well as sealability. This product has very low gel amount. The minimum biobased content of this grade is 87%, determined according to ASTM D6866.

Additive: Antiblocking High; Slip High

Applications: Automatic Packaging (FFS); liners; general purpose; HDPE and LDPE blends.

Information provided by Braskem

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.918 g/cc0.0332 lb/in³ASTM D792
Melt Flow 1.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
1.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 1070 %1070 %ASTM D882
Film Elongation at Break, TD 1340 %1340 %ASTM D882
Elmendorf Tear Strength MD 180 g180 gASTM D1922
Elmendorf Tear Strength TD 400 g400 gASTM D1922
Dart Drop Test 130 g0.287 lbF50; ASTM D1709
Film Tensile Strength at Break, MD 40.0 MPa5800 psiASTM D882
Film Tensile Strength at Break, TD 30.0 MPa4350 psiASTM D882
1% Secant Modulus, MD 210 MPa30500 psiFlexural; ASTM D1709
1% Secant Modulus, TD 230 MPa33400 psiFlexural; ASTM D1709
 
Processing PropertiesMetricEnglishComments
Processing Temperature 180 - 210 °C356 - 410 °FProfile

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Braskem Green PE SGD4960 Blow Molded High Density Polyethylene
Braskem Green PE SGM9450F Blow Film Extrusion and Cast Film Extrusion High Density Polyethylene
Braskem Green PE SEB853/72 Blown Film Extrusion Low Density Polyethylene
Braskem Green PE SEB853 Blown and Cast Film Extrusion Low Density Polyethylene
Braskem Green PE SBF0323HC Blown Film Extrusion Low Density Polyethylene

PBRASK2007 / 199889

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.