MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil LD 2023.BA Wire & Cable Low Density Polyethylene Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE)

Material Notes: Product Description: ExxonMobil™ LD 2023.BA Wire & Cable is a non-stabilized LDPE, designed for the production of Medium/High Voltage insulation using the direct peroxide addition. For cleanliness reasons, the material is specially controlled through on-line optical control systems. Sufficient antioxidant should be added to meet specific ageing requirements

Availability: Africa & Middle East and Europe

Additive:

  • Antiblock: No
  • Slip: No
  • Thermal Stabilizer: No
Applications:
  • MV/HV peroxide cross-linked insulation

Information provided by ExxonMobil

Key Words: LDPE LD 101BA Wire & Cable
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.923 g/cc0.0333 lb/in³ExxonMobil method
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
2.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 49
@Time 15.0 sec
49
@Time 0.00417 hour
ASTM D2240
Tensile Strength at Break 11.0 MPa1600 psiASTM D638
Tensile Strength, Yield 13.1 MPa1900 psiASTM D638
Elongation at Break 570 %570 %ASTM D638
Elongation at Yield 20 %20 %ASTM D638
Flexural Modulus, 1% Secant 290 MPa42000 psiASTM D790
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 7.60e+16 ohm-cm7.60e+16 ohm-cmASTM D257
Dielectric Constant 2.22.2ASTM D150
Dissipation Factor 0.00100.0010ASTM D150
 
Thermal PropertiesMetricEnglishComments
Melting Point 110 °C230 °FPeak Melting Point; ExxonMobil method

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil LDPE LD 100.BW Low Density Polyethylene Resin
ExxonMobil LD 8016.BA Low Density Polyethylene Resin (European Grade)
ExxonMobil LD 6821.LC Low Density Polyethylene Resin
ExxonMobil LD 358BW Low Density Polyethylene Resin (European Grade)
ExxonMobil LD 2025.BR Low Density Polyethylene Resin

PEX99254 / 175490

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.