MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 185,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

AISI 1018 Steel, cold drawn, quenched, and tempered, 19-32 mm (0.75-1.25 in) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: Supplied as killed, semikilled, rimmed, and capped steel. Good weldability, relatively soft and strengthen with cold work during forming or drawing. Widely used in cold forming operations such as heading, upsetting, and extrusion. Used in the as-rolled condition as bar, shapes, sheet, and strip.

Key Words: UNS G10180, AMS 5069, ASTM A29, ASTM A108, ASTM A510, ASTM A513, ASTM A519, ASTM A544, ASTM A545, ASTM A548, ASTM A549, ASTM A576, ASTM A659, AS 1442 K1018 (Australia), AS 1443 K1018, CSN 12020 (Czech), CSN 12022, AFNOR NF A33-101 AF42C20, DIN 1.0453, DIN C16.8, DGN B-301 1018 (Mexico), COPANT 331 1018 (Pan America), COPANT 333 1018, MIL SPEC MIL-S-11310 (CS1018), SAE J403, SAE J412, SAE J414, MST.T (Russia), ST.20A, ST.3, ST.3T, GOST M18S, GOST 23570 18ps, GOST 23570 18sp, GOST 5520 18K, GOST 5521 S, NBN 629 D37-2 (Belgium), NBN 630 E37-1, NBN 630 E37-2, NBN A21-221 C17KD, BDS 9801 S (Bulgaria), GB 715 ML3 (China), TS 302 Fe35.2 (Turkey), TS 346 Fe35, BS 970 080A17, DEF STAN95-1-1 C1018
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.87 g/cc0.284 lb/in³Typical for steel
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 163163
Hardness, Knoop 184184Converted from Brinell
Hardness, Rockwell B 8484Converted from Brinell
Hardness, Vickers 170170Converted from Brinell
Tensile Strength, Ultimate 565 MPa81900 psi
Tensile Strength, Yield 485 MPa70300 psi
Elongation at Break 20 %20 %in 50 mm
Reduction of Area 57 %57 %
Modulus of Elasticity 200 GPa29000 ksi
Bulk Modulus 159 GPa23100 ksiEstimated from elastic modulus
Poissons Ratio 0.290.29Typical for steel
Machinability 65 %65 %Based on 100% machinability for AISI 1212 steel.
Shear Modulus 78.0 GPa11300 ksiEstimated from elastic modulus
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000159 ohm-cm
@Temperature 0.000 °C
0.0000159 ohm-cm
@Temperature 32.0 °F
annealed condition
 0.0000219 ohm-cm
@Temperature 100 °C
0.0000219 ohm-cm
@Temperature 212 °F
annealed condition
 0.0000293 ohm-cm
@Temperature 200 °C
0.0000293 ohm-cm
@Temperature 392 °F
annealed condition
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.5 µm/m-°C
@Temperature 20.0 °C
6.39 µin/in-°F
@Temperature 68.0 °F
Typical steel
 12.2 µm/m-°C
@Temperature 0.000 - 300 °C
6.78 µin/in-°F
@Temperature 32.0 - 572 °F
Typical for steel
 13.9 µm/m-°C
@Temperature 0.000 - 500 °C
7.72 µin/in-°F
@Temperature 32.0 - 932 °F
Typical for steel
Specific Heat Capacity 0.486 J/g-°C
@Temperature >=100 °C
0.116 BTU/lb-°F
@Temperature >=212 °F
annealed
Thermal Conductivity 51.9 W/m-K360 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.14 - 0.20 %0.14 - 0.20 %
Iron, Fe 98.81 - 99.26 %98.81 - 99.26 %As remainder
Manganese, Mn 0.60 - 0.90 %0.60 - 0.90 %
Phosphorus, P <= 0.040 %<= 0.040 %
Sulfur, S <= 0.050 %<= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1018 Steel, cold drawn
AISI 1018 Steel, hot rolled, quenched, and tempered
AISI 1018 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
AISI 1018 Steel, as cold drawn, 16-22 mm (0.625-0.875 in) round
AISI 1018 Steel, as cold drawn, 22-32 mm (0.875-1.25 in) round

M1018D / 6812

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.