MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

INEOS Styrolution Novodur® 4000PG ABS
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded

Material Notes: Novodur Ultra 4000PG is an injection molding grade especially suitable for electroplating, providing enhanced heat resistance.

Information provided by Styrolution

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ISO 1183
Linear Mold Shrinkage 0.0050 - 0.0080 cm/cm0.0050 - 0.0080 in/inISO 294-4
Melt Flow 6.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
6.0 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 100 MPa14500 psiISO 2039-1
Tensile Strength, Yield 46.0 MPa6670 psiISO 527
Elongation at Yield 3.1 %3.1 %ISO 527
Tensile Modulus 2.40 GPa348 ksiISO 527
Flexural Strength 73.0 MPa10600 psiISO 178
Flexural Modulus 2.35 GPa341 ksiISO 178
Izod Impact, Notched (ISO)  10.0 kJ/m²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 180/A
 23.0 kJ/m²
@Temperature 23.0 °C
10.9 ft-lb/in²
@Temperature 73.4 °F
ISO 180/A
Charpy Impact, Notched  1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 2.00 J/cm²
@Temperature 23.0 °C
9.52 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmIEC 60093
Surface Resistance >= 1.00e+16 ohm>= 1.00e+16 ohmIEC 60093
Dielectric Constant 3.0
@Frequency 100 Hz
3.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 38.0 kV/mm
@Thickness 1.50 mm
965 kV/in
@Thickness 0.0591 in
Short Time; IEC 60243-1
Dissipation Factor  0.0065
@Frequency 100 Hz
0.0065
@Frequency 100 Hz
IEC 60250
 0.0085
@Frequency 1e+6 Hz
0.0085
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 90.0 µm/m-°C50.0 µin/in-°FISO 11359
Deflection Temperature at 0.46 MPa (66 psi) 103 °C217 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 98.0 °C208 °FISO 75
Vicat Softening Point 107 °C
@Load 5.10 kg
225 °F
@Load 11.2 lb
50°C/h; ISO 306
 
Processing PropertiesMetricEnglishComments
Melt Temperature 230 - 270 °C446 - 518 °FISO 294
Mold Temperature 70.0 °C158 °FISO 294
Injection Velocity 240 mm/sec9.45 in/secISO 294
Drying Temperature 80.0 °C
@Time 7200 - 14400 sec
176 °F
@Time 2.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ineos ABS NOVODUR® P2T ABS, Injection Grade
INEOS Styrolution Terluran® HH-106 Q109 Colored ABS
Aclo Accucomp ABS ABS802L High Impact Grade
Celanese Hostaform® S 9364 XAP2 ™ POM, Impact Modified
Avient Edgetek® AS-20CF/000 Acrylonitrile Butadiene Styrene (ABS), Carbon Fiber Reinforced

PLANX596 / 159686

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.