MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior Novamid® 1013G15 1 NA PA6-GF15
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Glass Fiber Filled

Material Notes: 15% Glass Reinforced, Injection Molding

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.23 g/cc0.0444 lb/in³dry; ISO 1183
Moisture Absorption 3.00 %3.00 %Sim. To ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cm0.0040 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.013 cm/cm0.013 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 70.0 MPa10200 psicond; ISO 527-1/-2
 130 MPa18900 psidry; ISO 527-1/-2
Elongation at Break 2.7 %2.7 %dry; ISO 527-1/-2
 8.7 %8.7 %cond; ISO 527-1/-2
Tensile Modulus 2.80 GPa406 ksicond; ISO 527-1/-2
 5.80 GPa841 ksidry; ISO 527-1/-2
Flexural Strength 115 MPa16700 psicond; ISO 178
 200 MPa29000 psidry; ISO 178
Flexural Modulus 2.90 GPa421 ksicond; ISO 178
 5.40 GPa783 ksidry; ISO 178
Charpy Impact Unnotched  3.90 J/cm²
@Temperature 23.0 °C
18.6 ft-lb/in²
@Temperature 73.4 °F
dry; ISO 179/1eU
 10.6 J/cm²
@Temperature 23.0 °C
50.4 ft-lb/in²
@Temperature 73.4 °F
cond; ISO 179/1eU
Charpy Impact, Notched  0.600 J/cm²
@Temperature 23.0 °C
2.86 ft-lb/in²
@Temperature 73.4 °F
dry; ISO 179/1eA
 1.40 J/cm²
@Temperature 23.0 °C
6.66 ft-lb/in²
@Temperature 73.4 °F
cond; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 6.00e+14 ohm-cm6.00e+14 ohm-cmdry; IEC 60093
Surface Resistance 8.00e+13 ohm8.00e+13 ohmcond; IEC 60093
Dielectric Constant  4.0
@Frequency 100 Hz
4.0
@Frequency 100 Hz
dry; IEC 60250
 4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
dry; IEC 60250
Dielectric Strength 27.0 kV/mm686 kV/indry; IEC 60243-1
Dissipation Factor  0.013
@Frequency 100 Hz
0.013
@Frequency 100 Hz
dry; IEC 60250
 0.023
@Frequency 1e+6 Hz
0.023
@Frequency 1e+6 Hz
dry; IEC 60250
Comparative Tracking Index 400 V400 Vdry; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 216 °C421 °Fdry; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 194 °C381 °Fdry; ISO 75-1/-2
Flammability, UL94 HB
@Thickness 0.800 mm
HB
@Thickness 0.0315 in
dry; IEC 60695-11-10

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Techmer ES HiFill® PP GF15 CC 15% Glass Filled
EMS-Grivory Grilon® BG-15 PA6-GF15
Envalior Akulon® K224-G3 PA6-GF15, Dry, 15% Glass Filled
Celanese Zytel® 73G15HSL BK363 PA6-GF15
Avient Maxxam® 6529-1001 Polypropylene (PP), Talc Filled

PDSM9871 / 161492

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.