MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Iran Petrochemical (PCC) Poliran SBR-1778 Styrene Butadiene Rubber  (discontinued **)
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Information provided by Iran Petrochemical Commercial Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Mooney Viscosity  48 - 62
@Temperature 100 °C
48 - 62
@Temperature 212 °F
Raw, ML+4; A 1107
 <= 64
@Temperature 100 °C
<= 64
@Temperature 212 °F
Compound, ML+4; A 1154
Ash <= 1.5 %<= 1.5 %A 1102
Collected Volatile Condensable Material <= 0.75 %<= 0.75 %A 1101
 
Chemical PropertiesMetricEnglishComments
Styrene Content 22.5 - 24.5 %22.5 - 24.5 %Bound; A 1106
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break >= 19.61 MPa>= 2844 psi35 minute cure; A 1154
Elongation at Break >= 430 %>= 430 %35 minute cure; A 1154
300% Modulus  7.55 - 10.5 MPa
@Strain 300 %
1100 - 1520 psi
@Strain 300 %
25 minute cure; A 1154
 9.61 - 12.6 MPa
@Strain 300 %
1390 - 1820 psi
@Strain 300 %
35 minute cure; A 1154
 10.9 - 13.8 MPa
@Strain 300 %
1580 - 2010 psi
@Strain 300 %
50 minute cure; A 1154
 
Descriptive Properties
Organic Acid3.9-5.7 wt %A 1106
Soap<0.5 wt%A 1106

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical SBR 1778 High Acrylonitrile Polymer

PIPC059 / 48287

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.