MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

The NanoSteel® Company SHS 8000 TWAS Iron Based Alloy, Cored Wire
Categories: Metal; Ferrous Metal; Alloy Steel; Other Engineering Material; Ceramic/Metallic Coating

Material Notes: Coating Description: SHS 8000 TWAS is a glass forming iron based alloy that forms a nanocomposite comprised of a mixed amorphous and nanoscale microstructure when sprayed as a coating. SHS 8000 features high wear resistance, elevated temperature erosion resistance and a unique high hardness/toughness combination.

    Key Performance Characteristics
  • Excels in elevated temperature environments where fly ash and bed ash erosion occurs
  • Superior bond strength without necessity of bond coat
  • Hardness increases as a function of time and temperature

Application Process: Twin Wire Arc Spraying (TWAS)

Information Provided by The NanoSteel Company, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.30 g/cc0.264 lb/in³Coating Property
Porosity <= 5.0 %<= 5.0 %Coating Property
 
Mechanical PropertiesMetricEnglishComments
Vickers Microhardness 1064 - 12341064 - 1234kg/mm2; HV300
 >= 117
@Temperature 760 °C
>= 117
@Temperature 1400 °F
 >= 309
@Temperature 649 °C
>= 309
@Temperature 1200 °F
 >= 620
@Temperature 316 °C
>= 620
@Temperature 600 °F
 >= 912
@Temperature 149 °C
>= 912
@Temperature 300 °F
 >= 1030
@Temperature 21.1 °C
>= 1030
@Temperature 70.0 °F
Adhesive Bond Strength 78.6 MPa
@Thickness 0.508 mm
11400 psi
@Thickness 0.0200 in
1018 steel; ASTM C633-01
Coefficient of Friction 0.3160.316
 
Thermal PropertiesMetricEnglishComments
CTE, linear 8.53 µm/m-°C
@Temperature 100 - 500 °C
4.74 µin/in-°F
@Temperature 212 - 932 °F
Thermal Conductivity  4.28 W/m-K
@Temperature 23.0 °C
29.7 BTU-in/hr-ft²-°F
@Temperature 73.4 °F
 4.678 W/m-K
@Temperature 50.0 °C
32.47 BTU-in/hr-ft²-°F
@Temperature 122 °F
 5.055 W/m-K
@Temperature 75.0 °C
35.08 BTU-in/hr-ft²-°F
@Temperature 167 °F
 5.269 W/m-K
@Temperature 100 °C
36.57 BTU-in/hr-ft²-°F
@Temperature 212 °F
 5.505 W/m-K
@Temperature 125 °C
38.20 BTU-in/hr-ft²-°F
@Temperature 257 °F
 5.707 W/m-K
@Temperature 150 °C
39.61 BTU-in/hr-ft²-°F
@Temperature 302 °F
 
Component Elements PropertiesMetricEnglishComments
Boron, B <= 5.0 %<= 5.0 %
Carbon, C <= 2.0 %<= 2.0 %
Chromium, Cr <= 22 %<= 22 %
Iron, Fe >= 59 %>= 59 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo <= 5.0 %<= 5.0 %
Niobium, Nb (Columbium, Cb) <= 5.0 %<= 5.0 %
Silicon, Si <= 1.0 %<= 1.0 %
 
Descriptive Properties
Impact ResistanceNo delamination/cracking at 480 in-lbsDrop Impact Testing
Wear Resistance Mass Loss (g)0.152000 cycles; ASTM G65-04 Procedure B

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Goodfellow Iron 77.5/Boron 15/Silicon 7.5 Alloy
AK Steel CARLITE® M-5 Grain Oriented Electrical Steel
AK Steel CARLITE® M-5 Grain Oriented Electrical Steel (Extended Electro-Magnetic Data)
Goodfellow Nickel/Iron/Silicon/Boron Alloy
Goodfellow Iron 40/Nickel 38/Boron 18 Alloy

NNANO008 / 106803

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.